MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay CYCOM® 985 Epoxy + Kevlar 49 Fiber Laminate
Categories: Polymer; Thermoset; Epoxy

Material Notes: CYCOM® 985 is a 350°F (177°C) curing epoxy resin system. CYCOM 985 is designed for use where a balance of performance and processing characteristics is required. It has excellent structural performance and good impact resistance. CYCOM 985 is co-curable with structural adhesives and will produce outstanding thin-skinned sandwich structures. CYCOM 985 allows thick section construction without exotherm problems. Optimum properties are achieved by curing under autoclave pressure from 45 to 100 psi (as appropriate to panel configuration) at 350°F (177°C) for two hours. CYCOM 985 prepregs have good tack and drape and an out-time of two weeks at room temperature.

Features & Benefits:

  • Modified epoxy system
  • Excellent hot/wet strength retention
  • 350°F (177°C) cure
  • Good impact resistance
  • 300°F (149°C) service temperature
  • Controlled flow
  • Ease of processing
  • Good tack and drape
  • 14 day shop life
  • Shelf life of 6 months at 0°F (-18°C)
Applications: Primary and secondary aircraft structures

Mechanical property data for 985 epoxy with 10 ply laminate with 50% fiber volume Kevlar 49 Fiber K-285.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.35 g/cc1.35 g/cc
 
Mechanical PropertiesMetricEnglishComments
Tensile Modulus  21.0 GPa
@Temperature 177 °C
3050 ksi
@Temperature 351 °F
 23.0 GPa
@Temperature 132 °C
3340 ksi
@Temperature 270 °F
 28.0 GPa
@Temperature 71.0 °C
4060 ksi
@Temperature 160 °F
 30.0 GPa
@Temperature 24.0 °C
4350 ksi
@Temperature 75.2 °F
 31.0 GPa
@Temperature -54.0 °C
4500 ksi
@Temperature -65.2 °F
Compressive Strength  165 MPa
@Temperature 24.0 °C
23900 psi
@Temperature 75.2 °F
Wet
 179 MPa
@Temperature 71.0 °C
26000 psi
@Temperature 160 °F
 214 MPa
@Temperature 24.0 °C
31000 psi
@Temperature 75.2 °F
 234 MPa
@Temperature -54.0 °C
33900 psi
@Temperature -65.2 °F
Compressive Modulus  26.0 GPa
@Temperature 177 °C
3770 ksi
@Temperature 351 °F
 29.0 GPa
@Temperature 24.0 °C
4210 ksi
@Temperature 75.2 °F
 30.0 GPa
@Temperature 71.0 °C
4350 ksi
@Temperature 160 °F
 30.0 GPa
@Temperature 132 °C
4350 ksi
@Temperature 270 °F
 30.0 GPa
@Temperature -54.0 °C
4350 ksi
@Temperature -65.2 °F
Shear Strength  10.3 MPa
@Temperature 177 °C
1500 psi
@Temperature 351 °F
Short Beam, wet
 13.8 MPa
@Temperature 177 °C
2000 psi
@Temperature 351 °F
Short Beam
 15.2 MPa
@Temperature 132 °C
2200 psi
@Temperature 270 °F
Short Beam, wet
 29.0 MPa
@Temperature -54.0 °C
4200 psi
@Temperature -65.2 °F
Short Beam
 29.6 MPa
@Temperature 132 °C
4300 psi
@Temperature 270 °F
Short Beam
 31.7 MPa
@Temperature 71.0 °C
4600 psi
@Temperature 160 °F
Short Beam, wet
 34.5 MPa
@Temperature 24.0 °C
5000 psi
@Temperature 75.2 °F
Short Beam, wet
 37.2 MPa
@Temperature 24.0 °C
5400 psi
@Temperature 75.2 °F
Short Beam
 40.0 MPa
@Temperature 71.0 °C
5800 psi
@Temperature 160 °F
Short Beam
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 149 °C300 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 177 °C
@Time 7200 sec
350 °F
@Time 2.00 hour
Cure
Shelf Life 6.00 Month
@Temperature -17.8 °C
6.00 Month
@Temperature 0.000 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont™ Kevlar® 49 Aramid Fiber
Hexcel® F161 Epoxy Resin, 120 Kevlar Fabric
G-10 Fiberglass Epoxy Laminate Sheet
Arlon Electronic Materials 45NK Woven Kevlar® Reinforced Laminate and Prepreg
Fibre Glast 549 Kevlar® Fabric

PCYTED092a / 234739

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.