RheTech Products FT4900-01UV Thermoplastic Polyolefin, UV Stabilized, Black
Categories:
Polymer
;
Thermoplastic
;
Polyolefin
Material Notes:
Applications:
Exterior components
Bodyside moldings
Step pads
License plate brackets
Injection molding conditions reported in table.
Information provided by RheTech Products.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
0.950
g/cc
@Temperature 23.0 °C
0.950
g/cc
@Temperature 73.4 °F
23/23°C; ASTM D792
Filler Content
8 %
8 %
ASTM D5630
Linear Mold Shrinkage
0.012
cm/cm
0.012
in/in
ASTM D955
Melt Flow
17
g/10 min
@Load 2.16 kg,
Temperature 230 °C
17
g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Hardness, Shore D
64
64
ASTM D2240
Tensile Strength at Break
18.6
MPa
2700
psi
2 in/min; ASTM D638
Flexural Modulus
1.10
GPa
160
ksi
Tangent; ASTM D790
Izod Impact, Notched
8.01
J/cm
@Temperature 23.0 °C
15.0
ft-lb/in
@Temperature 73.4 °F
ASTM D256
Gardner Impact
24.8
J
18.3
ft-lb
ASTM D5420
Thermal Properties
Metric
English
Comments
Deflection Temperature at 0.46 MPa (66 psi)
90.6
°C
195
°F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
56.7
°C
134
°F
ASTM D648
Processing Properties
Metric
English
Comments
Rear Barrel Temperature
193
-
221
°C
380
-
430
°F
Middle Barrel Temperature
199
-
227
°C
390
-
440
°F
Front Barrel Temperature
204
-
232
°C
400
-
450
°F
Nozzle Temperature
210
-
221
°C
410
-
430
°F
Mold Temperature
26.7
-
48.9
°C
80.0
-
120
°F
Drying Temperature
65.6
-
82.2
°C
150
-
180
°F
Dry Time
1
-
2
hour
1
-
2
hour
Moisture Content
<= 0.050 %
<= 0.050 %
Recommended
Injection Pressure
2.76
-
10.3
MPa
400
-
1500
psi
Hold Pressure
2.07
-
8.27
MPa
300
-
1200
psi
Back Pressure
0.345
-
1.03
MPa
50.0
-
150
psi
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
RheTech Products FT3080-727UV Thermoplastic Polyolefin, UV Stabilized, G01 Black
RheTech Products FT5250-650UV Thermoplastic Polyolefin, UV Stabilized, Exterior 848 Black
RheTech Products FT4900-74UV Thermoplastic Polyolefin, UV Stabilized, Exterior DX9 Black
RheTech Products FT4802-01UV Thermoplastic Polyolefin, UV Stabilized, Black
RTP Company RTP 107 CC UV Polypropylene (PP), Glass Fiber - Chemically Coupled - UV Stabilized
PRHET106 / 65674
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.