MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum A357.0-T62, Cast
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes:

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium A357.0-T62; UNS A13570; AAA357.0-T62; AlA357.0-T62
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.67 g/cc0.0965 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 310 MPa45000 psiClass 1
Tensile Strength, Yield 241 MPa35000 psiClass 1
Elongation at Break 3.0 %3.0 %in 4d
Tensile Modulus 72.4 GPa10500 ksiCompressive modulus in is typically about 2% higher for Al alloys
Compressive Yield Strength 241 MPa35000 psiClass 1
Poissons Ratio 0.330.33Calculated Value
Fatigue Strength  110 MPa
@# of Cycles 5.00e+8
16000 psi
@# of Cycles 5.00e+8
Notch Status unknown, R.R. Moore Test
 255 MPa
@# of Cycles 100000
37000 psi
@# of Cycles 100000
Notch status unknown, rotating beam
Machinability 50 %50 %0-100 Scale (100=best)
Shear Modulus 26.8 GPa3890 ksi
Shear Strength 187 MPa27100 psiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000440 ohm-cm0.00000440 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 389 J/g167 BTU/lbTypical for cast aluminum
CTE, linear  21.4 µm/m-°C
@Temperature 20.0 - 100 °C
11.9 µin/in-°F
@Temperature 68.0 - 212 °F
 23.2 µm/m-°C
@Temperature 20.0 - 300 °C
12.9 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.963 J/g-°C0.230 BTU/lb-°F
Thermal Conductivity 151 W/m-K1050 BTU-in/hr-ft²-°F
Melting Point 557 - 613 °C1030 - 1140 °F
Solidus 557 °C1030 °F
Liquidus 613 °C1140 °F
 
Processing PropertiesMetricEnglishComments
Solution Temperature 540.6 °C1005 °Fhold at temperature for 8 hr; hot water quench
Aging Temperature 171 °C340 °Fhold at temperature 3 to 5 hrs
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 90.7 - 93 %90.7 - 93 %As remainder
Beryllium, Be 0.04 - 0.07 %0.04 - 0.07 %
Copper, Cu <= 0.20 %<= 0.20 %
Iron, Fe <= 0.20 %<= 0.20 %
Magnesium, Mg 0.40 - 0.70 %0.40 - 0.70 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 6.5 - 7.5 %6.5 - 7.5 %
Titanium, Ti 0.04 - 0.20 %0.04 - 0.20 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Corundum, Aluminum Oxide, Alumina, 99.9%, Al2O3
Aluminum A357.0-T61, Permanent Mold Cast
Aluminum - SiC Metal Matrix Composite
Aluminum A356.0-T6, Sand Cast
Aluminum A357.2 Composition Spec

MAC3570A62 / 9946

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.