MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Teknor Apex Medalist® MD-160 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Uses: Medical/Healthcare Applications; Pharmaceuticals; Safety Equipment

Agency Ratings: ISO 10993 Part 5

Processing Method: Extrusion; Injection Molding

Forms: Pellets

Injection Notes: Drying is not necessary. However, if moisture is a problem, dry the pellets for 2 to 4 hours at 150°F (65°C).

Extrusion Notes: Screw Speed: 30 to 100 rpm

Information Provided by Teknor Apex

Key Words: TPE
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.890 g/cc0.890 g/ccASTM D792
Linear Mold Shrinkage 0.027 cm/cm0.027 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.021 cm/cm0.021 in/inASTM D955
Melt Flow 1.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
1.0 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6565ASTM D2240
Tensile Strength at Break 11.7 MPa1700 psiASTM D412
Tensile Stress at Strain  2.48 MPa
@Strain 100 %
360 psi
@Strain 100 %
ASTM D412
 3.45 MPa
@Strain 200 %
500 psi
@Strain 200 %
ASTM D412
 4.48 MPa
@Strain 300 %
650 psi
@Strain 300 %
ASTM D412
Elongation at Break 750 %750 %ASTM D412
Tear Strength 59.6 kN/m340 pliASTM D624
Compression Set 18 %
@Temperature 22.8 °C,
Time 79200 sec
18 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 127 - 149 °C260 - 300 °F
Middle Barrel Temperature 138 - 160 °C280 - 320 °F
Front Barrel Temperature 149 - 171 °C300 - 340 °F
Nozzle Temperature 171 - 193 °C340 - 380 °F
Zone 1 138 - 149 °C280 - 300 °F
Zone 2 149 - 160 °C300 - 320 °F
Zone 3 160 - 182 °C320 - 360 °F
Zone 5 171 - 193 °C340 - 380 °F
Die Temperature 182 - 204 °C360 - 400 °F
Melt Temperature 171 - 193 °C340 - 380 °FProcessing Temperature
Mold Temperature 21.1 - 37.8 °C70.0 - 100 °F
Injection Pressure 1.38 - 5.52 MPa200 - 800 psi
Back Pressure 0.172 - 0.689 MPa25.0 - 100 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
AppearanceTranslucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Medalist® MD-12160H Thermoplastic Elastomer
A. Schulman DuraGrip™ 6070 BK Thermoplastic Elastomer
Teknor Apex Medalist® MD-17270 Thermoplastic Elastomer
Teknor Apex Medalist® MD-150 Thermoplastic Elastomer
Teknor Apex Medalist® MD-12362 Thermoplastic Elastomer

PTEKNO709 / 128887

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.