AISI 1117 Steel, normalized at 900°C (1650°F), air cooled, round
Categories:
Metal
;
Ferrous Metal
;
Carbon Steel
;
AISI 1000 Series Steel
;
Low Carbon Steel
Material Notes:
Applications include medium duty shafts, studs, pins, distributor cams, cam shafts, and universal joints.
Key Words:
UNS G11170, ASTM A29, ASTM A107, ASTM A108, FED QQ-S-637 (C1117), MIL SPEC MIL-S-18411, SAE J403, SAE J412, SAE J414
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
7.87
g/cc
0.284
lb/in³
Typical for steel.
Mechanical Properties
Metric
English
Comments
Hardness, Brinell
126
@Diameter 102 mm
126
@Diameter 4.00 in
137
@Diameter 25.4 mm
137
@Diameter 1.00 in
137
@Diameter 50.8 mm
137
@Diameter 2.00 in
143
@Diameter 12.7 mm
143
@Diameter 0.500 in
Hardness, Knoop
145
@Diameter 102 mm
145
@Diameter 4.00 in
Converted from Brinell
156
@Diameter 25.4 mm
156
@Diameter 1.00 in
Converted from Brinell
156
@Diameter 50.8 mm
156
@Diameter 2.00 in
Converted from Brinell
163
@Diameter 12.7 mm
163
@Diameter 0.500 in
Converted from Brinell
Hardness, Rockwell B
71
@Diameter 102 mm
71
@Diameter 4.00 in
Converted from Brinell
75
@Diameter 25.4 mm
75
@Diameter 1.00 in
Converted from Brinell
75
@Diameter 50.8 mm
75
@Diameter 2.00 in
Converted from Brinell
78
@Diameter 12.7 mm
78
@Diameter 0.500 in
Converted from Brinell
Hardness, Vickers
131
@Diameter 102 mm
131
@Diameter 4.00 in
Converted from Brinell
143
@Diameter 25.4 mm
143
@Diameter 1.00 in
Converted from Brinell
143
@Diameter 50.8 mm
143
@Diameter 2.00 in
Converted from Brinell
149
@Diameter 12.7 mm
149
@Diameter 0.500 in
Converted from Brinell
Tensile Strength, Ultimate
440
MPa
@Diameter 102 mm
63800
psi
@Diameter 4.00 in
462
MPa
@Diameter 50.8 mm
67000
psi
@Diameter 2.00 in
467
MPa
@Diameter 25.4 mm
67700
psi
@Diameter 1.00 in
481
MPa
@Diameter 12.7 mm
69800
psi
@Diameter 0.500 in
Tensile Strength, Yield
241
MPa
@Diameter 102 mm
35000
psi
@Diameter 4.00 in
286
MPa
@Diameter 50.8 mm
41500
psi
@Diameter 2.00 in
303
MPa
@Diameter 25.4 mm
43900
psi
@Diameter 1.00 in
310
MPa
@Diameter 12.7 mm
45000
psi
@Diameter 0.500 in
Elongation at Break
33.5 %
@Diameter 25.4 mm
33.5 %
@Diameter 1.00 in
in 50 mm
33.5 %
@Diameter 50.8 mm
33.5 %
@Diameter 2.00 in
in 50 mm
34.3 %
@Diameter 102 mm
34.3 %
@Diameter 4.00 in
in 50 mm
34.3 %
@Diameter 12.7 mm
34.3 %
@Diameter 0.500 in
in 50 mm
Reduction of Area
61 %
@Diameter 12.7 mm
61 %
@Diameter 0.500 in
63.8 %
@Diameter 25.4 mm
63.8 %
@Diameter 1.00 in
64.7 %
@Diameter 50.8 mm
64.7 %
@Diameter 2.00 in
64.7 %
@Diameter 102 mm
64.7 %
@Diameter 4.00 in
Modulus of Elasticity
200
GPa
29000
ksi
Typical for steel
Bulk Modulus
160
GPa
23200
ksi
Typical for steel.
Poissons Ratio
0.29
0.29
Typical For Steel
Shear Modulus
80.0
GPa
11600
ksi
Typical for steel.
Izod Impact
85.0
J
62.7
ft-lb
normalized at 900°C (1650°F)
Electrical Properties
Metric
English
Comments
Electrical Resistivity
0.0000174
ohm-cm
0.0000174
ohm-cm
Typical steel
Thermal Properties
Metric
English
Comments
CTE, linear
11.5
µm/m-°C
@Temperature 20.0 °C
6.39
µin/in-°F
@Temperature 68.0 °F
Typical steel
12.2
µm/m-°C
@Temperature 0.000 - 300 °C
6.78
µin/in-°F
@Temperature 32.0 - 572 °F
Typical for steel
13.9
µm/m-°C
@Temperature 0.000 - 500 °C
7.72
µin/in-°F
@Temperature 32.0 - 932 °F
Typical for steel
Specific Heat Capacity
0.481
J/g-°C
@Temperature >=100 °C
0.115
BTU/lb-°F
@Temperature >=212 °F
condition unknown
Thermal Conductivity
51.9
W/m-K
360
BTU-in/hr-ft²-°F
Typical steel
Component Elements Properties
Metric
English
Comments
Carbon, C
0.14 - 0.20 %
0.14 - 0.20 %
Iron, Fe
98.33 - 98.78 %
98.33 - 98.78 %
As remainder
Manganese, Mn
1.0 - 1.3 %
1.0 - 1.3 %
Phosphorus, P
<= 0.040 %
<= 0.040 %
Sulfur, S
0.080 - 0.13 %
0.080 - 0.13 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
AISI Type 304N Stainless Steel
304 Stainless Steel
AISI 1040 Steel, oil quenched from 855°C (1570°F), 595°C (1100°F) temper, 25 mm (1 in.) round
AISI 1030 Steel, water quenched from 870°C (1600°F), 540°C (1000°F) temper, 13 mm (0.5 in.) round
AISI 1035 Steel, cold drawn, high temperature, stress relieved, 50-75 mm (2-3 in) round
M1117S / 7145
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.