MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

General Plastics LAST-A-FOAM® FR-7104 Polyurethane Foam
Categories: Other Engineering Material; Composite Core Material; Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane Foam, Unreinforced

Material Notes: Product Feature:
  • Will not warp or bow
  • Chemically inert
  • Dimensionally stable
  • Grain-free stock material
  • Fine-cell structures
  • Closed-cell
  • Easily bonded and finished with a wide variety of adhesives and coatings
  • Low densities can be hand carved and shaped easily with common woodworking tools
  • Higher densities are available for CNC work where more accuracy is desired
  • Custom sizes available
Applications:
  • Proof stock
  • Composite core
  • Prototype models
  • Styling models
  • Tooling aids
  • Check fixtures
  • Mold patterns
  • Foundry patterns
  • Decorative trim

Information provided by General Plastics Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.0640 g/cc0.00231 lb/in³ASTM D1622
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 3.53.5cut foam surface; ASTM D2240
Tensile Strength 0.634 MPa92.0 psiPerpendicular to Rise; ASTM D1623
 0.648 MPa94.0 psiParallel to Rise; ASTM D1623
Flexural Strength 0.689 MPa100 psiRise Parallel to Beam Thick.; ASTM D790
 0.696 MPa101 psiRise Parallel to Test Span; ASTM D790
Flexural Modulus 0.02102 GPa3.048 ksiRise Parallel to Beam Thick.; ASTM D790
 0.02112 GPa3.063 ksiRise Parallel to Test Span; ASTM D790
Compressive Strength  0.276 MPa
@Temperature 93.3 °C
40.0 psi
@Temperature 200 °F
Perpendicular to Rise; ASTM D1621
 0.296 MPa
@Temperature 93.3 °C
43.0 psi
@Temperature 200 °F
Parallel to Rise; ASTM D1621
 0.510 MPa
@Temperature 23.9 °C
74.0 psi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 0.758 MPa
@Temperature 23.9 °C
110 psi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
Compressive Modulus  0.009094 GPa
@Temperature 93.3 °C
1.319 ksi
@Temperature 200 °F
Perpendicular to Rise; ASTM D1621
 0.0111 GPa
@Temperature 93.3 °C
1.61 ksi
@Temperature 200 °F
Parallel to Rise; ASTM D1621
 0.01324 GPa
@Temperature 23.9 °C
1.921 ksi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 0.01631 GPa
@Temperature 23.9 °C
2.365 ksi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
Poissons Ratio 0.300.30
 
Thermal PropertiesMetricEnglishComments
CTE, linear 55.8 µm/m-°C
@Temperature -45.6 - 93.3 °C
31.0 µin/in-°F
@Temperature -50.0 - 200 °F
GP Method
Thermal Conductivity 0.0272 W/m-K0.189 BTU-in/hr-ft²-°FASTM C518
Glass Transition Temp, Tg 119 °C246 °FASTM E1824
 
Descriptive Properties
Tumbling Friability (%)8.220 mins at 60 rpm, ASTM C421
Water Absorption0.019 lbs/ft²ASTM D2842

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
General Plastics LAST-A-FOAM® FR-10106 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-10108 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-3818 FST Polyurethane Foam
General Plastics LAST-A-FOAM® FR-7105 Polyurethane Foam
General Plastics LAST-A-FOAM® FR-7107 Polyurethane Foam

PGENR043 / 186829

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.