MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

TriSteel

Saint-Gobain Fluoroloy® A16 High Performance Seal Material
Categories: Polymer; Thermoplastic

Material Notes: General purpose material for heat and wear resistance; Recommended for dry and poorly lubricated applications; Particularly suitable for water and steam service

Information provided by Saint-Gobain Performance Plastics.

Vendors: TriStar Plastics Corp. provides engineering, custom fabrication and manufacturing of high-performance plastics and self-lubricating bearing materials, such as Fluoroloy®, Rulon, PEEK, Torlon, CJ Composites and Ultracomp. Capabilities include component design, material selection, prototype and production, manufacturing and surface modification. Call (800) TRI-STAR (800) 874-7827 or visit or www.TStar.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.13 g/cc0.0770 lb/in³ASTM D792
Deformation 7.0 %
@Time 86400 sec
7.0 %
@Time 24.0 hour
13.8 MPa (2000 psi) load; ASTM D621
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6060ASTM D2240
Tensile Strength 20.7 MPa3000 psiASTM D4894
Elongation at Break 200 %200 %ASTM D4894
Tensile Modulus 0.386 GPa56.0 ksiASTM D4894
Compressive Yield Strength 13.1 MPa
@Strain 1 %
1900 psi
@Strain 1 %
ASTM D695
Compressive Modulus 0.758 GPa110 ksiASTM D695
Coefficient of Friction 0.090.09
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 129 µm/m-°C
@Temperature 26.0 - 200 °C
71.7 µin/in-°F
@Temperature 78.8 - 392 °F
Mold Direction; ASTM D696
CTE, linear, Transverse to Flow 126 µm/m-°C
@Temperature 26.0 - 200 °C
70.0 µin/in-°F
@Temperature 78.8 - 392 °F
ASTM D696
Maximum Service Temperature, Air 260 °C500 °F
Minimum Service Temperature, Air -268 °C-450 °F
 
Descriptive Properties
ColorDark Gray

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Saint-Gobain Fluoroloy® A08 High Performance Seal Material
Saint-Gobain Fluoroloy® A09 High Performance Seal Material
Saint-Gobain Fluoroloy® A22 High Performance Seal Material
Saint-Gobain Fluoroloy® A12 High Performance Seal Material
Saint-Gobain Fluoroloy® A01 High Performance Seal Material

PSTGQ965 / 150504

TriSteel

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.