MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Leaded Yellow Brass, UNS C85800, Copper Casting Alloy, Die Castings
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass; Copper Casting Alloy

Material Notes:

Casting methods recommended for this alloy: Die.

Applications: General purpose die casting alloy having moderate strength.

Classified under: Yellow brasses and leaded yellow brasses. ASTM B176; formerly ASTM Z30A

Typical data for die castings, separately cast test bars.. Alloy does not respond to heat treating. Casting shrinkage allowance is 2%

Key Words: leaded yellow brass, 63-1-1-35, CA 858, ASTM B30, ASTM B176 (CA858), ASTM B176, ASTM Z30A, SAE J462, Ingot code no. 406, MIL-C-15345 (Alloy 3)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.41 g/cc0.304 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 102102
Tensile Strength, Ultimate 380 MPa55100 psi
Tensile Strength, Yield 205 MPa
@Strain 0.5 %
29700 psi
@Strain 0.5 %
Elongation at Break 15 %15 %In 50 mm
Modulus of Elasticity 105 GPa15200 ksi
Machinability 80 %80 %UNS C36000 (free-cutting brass) = 100%
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000078368 ohm-cm
@Temperature 20.0 °C
0.0000078368 ohm-cm
@Temperature 68.0 °F
22% IACS
Magnetic Permeability 1.01.0
 
Thermal PropertiesMetricEnglishComments
CTE, linear 22.0 µm/m-°C
@Temperature 20.0 - 260 °C
12.2 µin/in-°F
@Temperature 68.0 - 500 °F
Specific Heat Capacity 0.376 J/g-°C0.0899 BTU/lb-°F
Thermal Conductivity 83.9 W/m-K
@Temperature 20.0 °C
582 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 903 - 920 °C1660 - 1690 °F
Solidus 903 °C1660 °F
Liquidus 920 °C1690 °F
Shrinkage 1.6 %1.6 %Patternmaker's Shrinkage (3/16 in./ft.)
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu >= 58 %>= 58 %
Iron, Fe <= 0.50 %<= 0.50 %
Lead, Pb <= 1.5 %<= 1.5 %
Manganese, Mn <= 0.25 %<= 0.25 %
Other, total <= 0.50 %<= 0.50 %
Tin, Sn <= 1.5 %<= 1.5 %
Zinc, Zn 35 %35 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Free-Cutting Brass, UNS C36000
Extra-high-leaded brass, UNS C35600
Leaded Yellow Brass, UNS C85700, Copper Casting Alloy, Sand and Centrifugal Castings
Chicago Extruded Metals UNS C38500 Copper-Zinc-Lead Alloy

MC85800b1 / 11911

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.