MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Moplen HP400L Polypropylene Homopolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Description: All ingredients in HP400L meet the chemical registration requirements of TSCA (U.S.) and DSL (Canada). Uses: Toys, containers, lids, medical applications, closure caps

Information provided by Basell.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ASTM D792 & ISO 1183
Melt Flow  5.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
5.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 6.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
6.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
Condition L; ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 8989ASTM D 785
Hardness, Shore D 7373ISO 868
Tensile Strength, Yield 32.0 MPa4640 psiISO 527-1, 2
 35.2 MPa5100 psiASTM D 638
Elongation at Yield 10 %10 %ASTM D 638
Flexural Modulus, 1% Secant 1590 MPa230000 psi0.05 in/min; ASTM D790
Izod Impact, Notched 0.427 J/cm0.800 ft-lb/in73°F; ASTM D256
 0.763 J/cm1.43 ft-lb/in73°F, Type 1, Notch A; ISO 180
Izod Impact, Notched (ISO) 3.00 kJ/m²1.43 ft-lb/in²Type 1, Notch A; ISO 180
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 93.3 °C200 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 51.1 °C124 °FUnannealed; ISO 75A-1, -2
Vicat Softening Point 155 °C311 °FMethod A; ISO 306
UL RTI, Electrical 221 °C
@Thickness 0.711 mm
430 °F
@Thickness 0.0280 in
UL 746
UL RTI, Mechanical with Impact 221 °C
@Thickness 0.711 mm
430 °F
@Thickness 0.0280 in
UL 746
UL RTI, Mechanical without Impact 221 °C
@Thickness 0.711 mm
430 °F
@Thickness 0.0280 in
UL 746
Flammability, UL94 HB
@Thickness 0.711 mm
HB
@Thickness 0.0280 in
NC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Moplen HP400N Polypropylene Homopolymer
Overview of materials for Polypropylene, Molded
LyondellBasell Moplen HP644H Polypropylene
LyondellBasell Moplen HP550J Polypropylene Homopolymer

PMO842 / 53831

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.