MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Aluminum 3003-H12
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 3000 Series Aluminum Alloy

Material Notes: Good weldability/formability and very good corrosion resistance lead to applications such as food and chemical handling, tanks, trim, litho sheet, pressure vessels, and piping.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A93003; ISO AlMn1Cu; Aluminium 3003-H12; AA3003-H12; Al3003-H12
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.73 g/cc0.0986 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 3535AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 131 MPa19000 psiAA; Typical
 115 - 160 MPa
@Thickness 0.432 - 50.8 mm
16700 - 23200 psi
@Thickness 0.0170 - 2.00 in
Tensile Strength, Yield 124 MPa18000 psiAA; Typical
 >= 83.0 MPa
@Thickness 0.432 - 50.8 mm
>= 12000 psi
@Thickness 0.0170 - 2.00 in
Elongation at Break  3.0 - 10 %
@Thickness 0.432 - 50.8 mm
3.0 - 10 %
@Thickness 0.0170 - 2.00 in
 10 %
@Thickness 1.59 mm
10 %
@Thickness 0.0625 in
AA; Typical
 20 %
@Diameter 12.7 mm
20 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Ultimate Bearing Strength 228 MPa33100 psiEdge distance/pin diameter = 2.0
Bearing Yield Strength 131 MPa19000 psiEdge distance/pin diameter = 2.0
Poissons Ratio 0.330.33
Fatigue Strength 55.2 MPa
@# of Cycles 5.00e+8
8000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 10 %10 %0-100 Scale of Aluminum Alloys
Shear Modulus 25.0 GPa3630 ksi
Shear Strength 82.7 MPa12000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000416 ohm-cm
@Temperature 20.0 °C
0.00000416 ohm-cm
@Temperature 68.0 °F
AA; Typical
Magnetic Susceptibility 8.0e-78.0e-7cgs/g at 25ºC
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.5 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.9 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.2 µm/m-°C
@Temperature 20.0 - 100 °C
12.9 µin/in-°F
@Temperature 68.0 - 212 °F
 23.2 µm/m-°C
@Temperature 20.0 - 100 °C
12.9 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.1 µm/m-°C
@Temperature 20.0 - 200 °C
13.4 µin/in-°F
@Temperature 68.0 - 392 °F
 25.1 µm/m-°C
@Temperature 20.0 - 300 °C
13.9 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.893 J/g-°C0.213 BTU/lb-°F
Thermal Conductivity 163 W/m-K1130 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 643 - 654 °C1190 - 1210 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 643 °C1190 °FAA; Typical
Liquidus 654 °C1210 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °FCommercial practice: 750 to 1100°F, higher temperatures used only for flash annealing.
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 96.7 - 99 %96.7 - 99 %As remainder
Copper, Cu 0.05 - 0.20 %0.05 - 0.20 %
Iron, Fe <= 0.70 %<= 0.70 %
Manganese, Mn 1.0 - 1.5 %1.0 - 1.5 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.60 %<= 0.60 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 3003-H14
Aluminum 3003-O
Aluminum 3003-H18
Aluminum 6061-T6; 6061-T651
Aluminum 5052-H32

MA3003H12 / 8980

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.