MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LG Chemical RS-650 ABS, Extrusion, General Purpose  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Extruded

Material Notes: Information Provided by LG Chem

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ISO 1183
Water Absorption 0.30 %0.30 %ISO 62
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inISO 2577
Melt Index of Compound 6.825 g/10 min
@Load 10.0 kg,
Temperature 220 °C
6.825 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 52.0 MPa7540 psi50 mm/min; ISO 527
Elongation at Break 30 %30 %50 mm/min; ISO 527
Elongation at Yield 5.0 %5.0 %50 mm/min; ISO 527
Tensile Modulus 2.30 GPa334 ksi1 mm/min; ISO 527
Flexural Yield Strength 76.0 MPa11000 psi2 mm/min; ISO 178
Flexural Modulus 2.50 GPa363 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO)  16.0 kJ/m²
@Temperature -30.0 °C
7.61 ft-lb/in²
@Temperature -22.0 °F
ISO 180
 34.0 kJ/m²
@Temperature 23.0 °C
16.2 ft-lb/in²
@Temperature 73.4 °F
ISO 80
Charpy Impact Unnotched  NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched  1.90 J/cm²
@Temperature -30.0 °C
9.04 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 3.60 J/cm²
@Temperature 23.0 °C
17.1 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 93
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 93
Dielectric Constant  2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
IEC 250
 3.0
@Frequency 100 Hz
3.0
@Frequency 100 Hz
IEC 250
Dielectric Strength 47.0 kV/mm1190 kV/inIEC 243
Dissipation Factor 0.0090
@Frequency 1e+6 Hz
0.0090
@Frequency 1e+6 Hz
IEC 250
Comparative Tracking Index 525 V525 VIEC 112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 80.0 µm/m-°C
@Temperature 20.0 °C
44.4 µin/in-°F
@Temperature 68.0 °F
ISO 11359
CTE, linear, Transverse to Flow 87.0 µm/m-°C
@Temperature 20.0 °C
48.3 µin/in-°F
@Temperature 68.0 °F
ISO 11359
Deflection Temperature at 0.46 MPa (66 psi) 98.0 °C208 °FAnnealed, 80°C, 4 hours; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °C203 °FAnnealed, 80°C, 4 hours; ISO 175
Vicat Softening Point 99.0 °C210 °F50 N, 50°C/h; ISO 306
Flammability, UL94  HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 220 - 250 °C428 - 482 °F
Mold Temperature 40.0 - 80.0 °C104 - 176 °F
Drying Temperature 75.0 - 85.0 °C167 - 185 °F
Dry Time 2 - 4 hour2 - 4 hourPredrying

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elix Polymers ELIX ABS E211 LNS013 Acrylonitrile Butadiene Styrene (ABS), Extrusion, Impact Grade
Asahi Kasei Stylac™ AE850 ABS Polymer, Extrusion, High Molding
Asahi Kasei Stylac™ AE510 ABS Polymer, Extrusion, High Molding
Asahi Kasei Stylac™ AE490 ABS Polymer, Extrusion, High Molding
Asahi Kasei Stylac™ A4130 ABS Polymer, Extrusion

PLGCHEM207 / 51028

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.