System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
LG Chemical Lupox® GP2156FT PBT+GF15%
(discontinued **)
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled
Material Notes:
Description: Injection Molding, PBT+GF15%, Flame Retardant, High Flow
Application: IT/OA, E&E (Connector)
CAS No. 71342-77-3, 65997-17-3, 24968-12-5 and 1309-64-4
Information provided by LG Chemical
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.52
g/cc
1.52
g/cc
ASTM D792
Maximum Moisture Content
0.020
0.020
Injection Molding
Linear Mold Shrinkage, Flow
0.0040
-
0.010
cm/cm
@Thickness 3.20 mm
0.0040
-
0.010
in/in
@Thickness 0.126 in
ASTM D955
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
98.1
MPa
@Thickness 3.20 mm
14200
psi
@Thickness 0.126 in
50mm/min; ASTM D638
Elongation at Break
3.0 %
@Thickness 3.20 mm
3.0 %
@Thickness 0.126 in
5mm/min; ASTM D638
Flexural Yield Strength
147
MPa
@Thickness 3.20 mm
21300
psi
@Thickness 0.126 in
1.3mm/min; ASTM D790
Flexural Modulus
5.88
GPa
@Thickness 3.20 mm
853
ksi
@Thickness 0.126 in
1.3mm/min; ASTM D790
Izod Impact, Notched
0.539
J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
1.01
ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+17
ohm-cm
1.00e+17
ohm-cm
ASTM D257
Dielectric Strength
26.0
kV/mm
@Thickness 1.00 mm
660
kV/in
@Thickness 0.0394 in
ASTM D149
Arc Resistance
0.00
-
60
sec
0.00
-
60
sec
ASTM D495
Comparative Tracking Index
175
V
175
V
Solution A; IEC 60112
Hot Wire Ignition, HWI
15
-
30
sec
@Thickness >=0.710 mm
15
-
30
sec
@Thickness >=0.0280 in
15
-
30
sec
@Thickness >=1.50 mm
15
-
30
sec
@Thickness >=0.0591 in
30
-
60
sec
@Thickness >=3.30 mm
30
-
60
sec
@Thickness >=0.130 in
High Amp Arc Ignition, HAI
>=
120
arcs
@Thickness 0.710 mm
>=
120
arcs
@Thickness 0.0280 in
>=
120
arcs
@Thickness 1.50 mm
>=
120
arcs
@Thickness 0.0591 in
>=
120
arcs
@Thickness 3.30 mm
>=
120
arcs
@Thickness 0.130 in
High Voltage Arc-Tracking Rate, HVTR
80.0
-
150
mm/min
3.15
-
5.91
in/min
Thermal Properties
Metric
English
Comments
Melting Point
225
°C
437
°F
@ Break; ASTM D3418
Deflection Temperature at 0.46 MPa (66 psi)
210
°C
@Thickness 6.40 mm
410
°F
@Thickness 0.252 in
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
200
°C
@Thickness 6.40 mm
392
°F
@Thickness 0.252 in
Unannealed; ASTM D648
UL RTI, Electrical
130
°C
@Thickness >=0.710 mm
266
°F
@Thickness >=0.0280 in
130
°C
@Thickness >=1.50 mm
266
°F
@Thickness >=0.0591 in
130
°C
@Thickness >=3.00 mm
266
°F
@Thickness >=0.118 in
UL RTI, Mechanical with Impact
130
°C
@Thickness >=0.710 mm
266
°F
@Thickness >=0.0280 in
130
°C
@Thickness >=1.50 mm
266
°F
@Thickness >=0.0591 in
130
°C
@Thickness >=3.00 mm
266
°F
@Thickness >=0.118 in
UL RTI, Mechanical without Impact
130
°C
@Thickness >=0.710 mm
266
°F
@Thickness >=0.0280 in
130
°C
@Thickness >=1.50 mm
266
°F
@Thickness >=0.0591 in
130
°C
@Thickness >=3.00 mm
266
°F
@Thickness >=0.118 in
Flammability, UL94
V-0
@Thickness >=0.710 mm
V-0
@Thickness >=0.0280 in
V-0
@Thickness >=1.50 mm
V-0
@Thickness >=0.0591 in
V-0
@Thickness >=3.00 mm
V-0
@Thickness >=0.118 in
Processing Properties
Metric
English
Comments
Rear Barrel Temperature
235
-
250
°C
455
-
482
°F
Injection Molding
Middle Barrel Temperature
240
-
250
°C
464
-
482
°F
Injection Molding
Front Barrel Temperature
245
-
255
°C
473
-
491
°F
Injection Molding
Nozzle Temperature
245
-
255
°C
473
-
491
°F
Injection Molding
Melt Temperature
245
-
255
°C
473
-
491
°F
Injection Molding
Mold Temperature
60.0
-
100
°C
140
-
212
°F
Injection Molding
Drying Temperature
120
°C
248
°F
Injection Molding
Dry Time
4.00
-
5.00
hour
4.00
-
5.00
hour
Injection Molding
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
LG Chemical Lupox® GP2100 PBT+GF10%
LG Chemical Lupox® TE5100 PBT+PC+GF10%
LG Chemical Lupox® HI2100M PBT+GF10%
LG Chemical Lupox® GP2156FL PBT+GF15%
Celanese Crastin® SK603 BK851 PBT-GF20
PLAY309 / 148319
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.