System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Celanese VECTRA A725 LCP, 25% Specialty
Categories:
Polymer
;
Thermoplastic
;
Liquid Crystal Polymer (LCP)
;
Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled
Material Notes:
Conductive Vectra grade, smooth surface compared to A700. 25% filled grade.
Information provided by Celanese
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.56
g/cc
0.0564
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.0030
cm/cm
0.0030
in/in
ISO 294-4
Linear Mold Shrinkage, Transverse
0.0080
cm/cm
0.0080
in/in
ISO 294-4
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell M
44
44
ISO 2039-2
Tensile Strength at Break
92.0
MPa
13300
psi
5mm/min; ISO 527-2/1A
Elongation at Break
4.2 %
4.2 %
5mm/min; ISO 527-2/1A
Tensile Modulus
8.10
GPa
1170
ksi
50mm/min; ISO 527-2/1A
Flexural Strength
124
MPa
18000
psi
ISO 178
Flexural Modulus
7.80
GPa
1130
ksi
ISO 178
Izod Impact, Notched (ISO)
17.0
kJ/m²
8.09
ft-lb/in²
ISO 180/1A
22.0
kJ/m²
@Temperature 23.0 °C
10.5
ft-lb/in²
@Temperature 73.4 °F
ISO 180/1U
Charpy Impact Unnotched
3.10
J/cm²
14.8
ft-lb/in²
ISO 179/1eU
Charpy Impact, Notched
1.70
J/cm²
8.09
ft-lb/in²
ISO 179/1eA
Electrical Properties
Metric
English
Comments
Volume Resistivity
1e+05
1e+05
IEC 60093
Surface Resistance
1.00e+6
ohm
1.00e+6
ohm
IEC 60093
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
10.0
µm/m-°C
5.56
µin/in-°F
ISO 11359-2
CTE, linear, Transverse to Flow
31.0
µm/m-°C
17.2
µin/in-°F
ISO 11359-2
Melting Point
280
°C
536
°F
10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 1.8 MPa (264 psi)
160
°C
320
°F
ISO 75-1, -2
Deflection Temperature at 8.0 MPa
93.0
°C
199
°F
ISO 75-1, -2
Flammability, UL94
V-0
V-0
Processing Properties
Metric
English
Comments
Processing Temperature
80.0
-
120
°C
176
-
248
°F
cavity
285
-
295
°C
545
-
563
°F
hot runner
Feed Temperature
60.0
-
80.0
°C
140
-
176
°F
Zone 1
270
-
280
°C
518
-
536
°F
Zone 2
275
-
285
°C
527
-
545
°F
Zone 3
280
-
290
°C
536
-
554
°F
Zone 4
285
-
295
°C
545
-
563
°F
Die Temperature
290
-
300
°C
554
-
572
°F
Melt Temperature
285
-
295
°C
545
-
563
°F
293
°C
559
°F
ISO 294
Mold Temperature
60.0
°C
140
°F
ISO 294
Injection Velocity
150
mm/sec
5.91
in/sec
ISO 294
Drying Temperature
>=
150
°C
>=
302
°F
Dry Time
4.00
-
6.00
hour
4.00
-
6.00
hour
Moisture Content
<= 0.010 %
<= 0.010 %
Injection Pressure
50.0
-
150
MPa
7250
-
21800
psi
Hold Pressure
48.0
MPa
6960
psi
ISO 294
50.0
-
150
MPa
7250
-
21800
psi
Back Pressure
<=
3.00
MPa
<=
435
psi
Screw Speed
80
rpm
@Diameter 40.0 mm
80
rpm
@Diameter 1.57 in
140
rpm
@Diameter 25.0 mm
140
rpm
@Diameter 0.984 in
200
rpm
@Diameter 16.0 mm
200
rpm
@Diameter 0.630 in
Descriptive Properties
Injection molding
Yes
Injection speed
very fast
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Celanese VECTRA A625 LCP, 25% Graphite Filled
Celanese Vectra® A422 Liquid Crystal Polymer (LCP), Glass/Graphite Filled
Celanese Hostaform® S 9364 POM, Impact Modified
Celanese VECTRA A430 LCP, 25% Specialty
Celanese VECTRA A435 LCP, 35% Specialty
PHCQ493 / 178948
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.