Physical Properties | Metric | English | Comments |
---|
Density | 8.60 g/cc | 0.311 lb/in³ |
| 8.64 g/cc | 0.312 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell B | 88 | 88 |
| 92 | 92 |
Tensile Strength, Ultimate | 628 MPa @Temperature 600 °C | 91100 psi @Temperature 1110 °F |
| 652 MPa @Temperature 500 °C | 94600 psi @Temperature 932 °F |
| 677 MPa @Temperature 400 °C | 98200 psi @Temperature 752 °F |
| 695 MPa @Temperature 300 °C | 101000 psi @Temperature 572 °F |
| 721 MPa @Temperature 200 °C | 105000 psi @Temperature 392 °F |
| 767 MPa @Temperature 100 °C | 111000 psi @Temperature 212 °F |
| 806 MPa @Temperature 25.0 °C | 117000 psi @Temperature 77.0 °F |
Tensile Strength, Yield | 223 MPa @Strain 0.2 %, Temperature 600 °C | 32300 psi @Strain 0.2 %, Temperature 1110 °F |
| 241 MPa @Strain 0.2 %, Temperature 500 °C | 35000 psi @Strain 0.2 %, Temperature 932 °F |
| 255 MPa @Strain 0.2 %, Temperature 400 °C | 37000 psi @Strain 0.2 %, Temperature 752 °F |
| 263 MPa @Strain 0.2 %, Temperature 300 °C | 38100 psi @Strain 0.2 %, Temperature 572 °F |
| 288 MPa @Strain 0.2 %, Temperature 200 °C | 41800 psi @Strain 0.2 %, Temperature 392 °F |
| 329 MPa @Strain 0.2 %, Temperature 100 °C | 47700 psi @Strain 0.2 %, Temperature 212 °F |
| 376 MPa @Strain 0.2 %, Temperature 25.0 °C | 54500 psi @Strain 0.2 %, Temperature 77.0 °F |
Elongation at Break | 62.3 % @Temperature 25.0 °C | 62.3 % @Temperature 77.0 °F |
| 65.9 % @Temperature 200 °C | 65.9 % @Temperature 392 °F |
| 66.7 % @Temperature 100 °C | 66.7 % @Temperature 212 °F |
| 68.8 % @Temperature 300 °C | 68.8 % @Temperature 572 °F |
| 69.3 % @Temperature 500 °C | 69.3 % @Temperature 932 °F |
| 69.5 % @Temperature 400 °C | 69.5 % @Temperature 752 °F |
| 70.6 % @Temperature 600 °C | 70.6 % @Temperature 1110 °F |
Reduction of Area | 69.1 % @Temperature 600 °C | 69.1 % @Temperature 1110 °F |
| 70.9 % @Temperature 500 °C | 70.9 % @Temperature 932 °F |
| 73 % @Temperature 400 °C | 73 % @Temperature 752 °F |
| 75.2 % @Temperature 300 °C | 75.2 % @Temperature 572 °F |
| 77.3 % @Temperature 200 °C | 77.3 % @Temperature 392 °F |
| 77.5 % @Temperature 25.0 °C | 77.5 % @Temperature 77.0 °F |
| 78 % @Temperature 100 °C | 78 % @Temperature 212 °F |
Modulus of Elasticity | 181 GPa @Temperature 600 °C | 26300 ksi @Temperature 1110 °F |
| 195 GPa @Temperature 500 °C | 28300 ksi @Temperature 932 °F |
| 205 GPa @Temperature 400 °C | 29700 ksi @Temperature 752 °F |
| 209 GPa @Temperature 300 °C | 30300 ksi @Temperature 572 °F |
| 211 GPa @Temperature 200 °C | 30600 ksi @Temperature 392 °F |
| 218 GPa @Temperature 100 °C | 31600 ksi @Temperature 212 °F |
| 223 GPa @Temperature 25.0 °C | 32300 ksi @Temperature 77.0 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000980 ohm-cm @Temperature 25.0 °C | 0.0000980 ohm-cm @Temperature 77.0 °F |
| 0.000100 ohm-cm @Temperature 100 °C | 0.000100 ohm-cm @Temperature 212 °F |
| 0.000104 ohm-cm @Temperature 200 °C | 0.000104 ohm-cm @Temperature 392 °F |
| 0.000108 ohm-cm @Temperature 300 °C | 0.000108 ohm-cm @Temperature 572 °F |
| 0.000112 ohm-cm @Temperature 400 °C | 0.000112 ohm-cm @Temperature 752 °F |
| 0.000115 ohm-cm @Temperature 500 °C | 0.000115 ohm-cm @Temperature 932 °F |
| 0.000117 ohm-cm @Temperature 600 °C | 0.000117 ohm-cm @Temperature 1110 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 11.6 µm/m-°C @Temperature 25.0 - 100 °C | 6.44 µin/in-°F @Temperature 77.0 - 212 °F |
| 12.0 µm/m-°C @Temperature 25.0 - 200 °C | 6.67 µin/in-°F @Temperature 77.0 - 392 °F |
| 12.4 µm/m-°C @Temperature 25.0 - 300 °C | 6.89 µin/in-°F @Temperature 77.0 - 572 °F |
| 12.7 µm/m-°C @Temperature 25.0 - 400 °C | 7.06 µin/in-°F @Temperature 77.0 - 752 °F |
| 13.1 µm/m-°C @Temperature 25.0 - 500 °C | 7.28 µin/in-°F @Temperature 77.0 - 932 °F |
| 13.3 µm/m-°C @Temperature 25.0 - 600 °C | 7.39 µin/in-°F @Temperature 77.0 - 1110 °F |
Specific Heat Capacity | 0.412 J/g-°C @Temperature 25.0 °C | 0.0985 BTU/lb-°F @Temperature 77.0 °F |
| 0.434 J/g-°C @Temperature 100 °C | 0.104 BTU/lb-°F @Temperature 212 °F |
| 0.451 J/g-°C @Temperature 200 °C | 0.108 BTU/lb-°F @Temperature 392 °F |
| 0.465 J/g-°C @Temperature 300 °C | 0.111 BTU/lb-°F @Temperature 572 °F |
| 0.477 J/g-°C @Temperature 400 °C | 0.114 BTU/lb-°F @Temperature 752 °F |
| 0.488 J/g-°C @Temperature 500 °C | 0.117 BTU/lb-°F @Temperature 932 °F |
| 0.504 J/g-°C @Temperature 600 °C | 0.120 BTU/lb-°F @Temperature 1110 °F |
Thermal Conductivity | 11.8 W/m-K @Temperature 25.0 °C | 81.9 BTU-in/hr-ft²-°F @Temperature 77.0 °F |
| 13.5 W/m-K @Temperature 100 °C | 93.7 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 15.4 W/m-K @Temperature 200 °C | 107 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 17.1 W/m-K @Temperature 300 °C | 119 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 18.6 W/m-K @Temperature 400 °C | 129 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 20.5 W/m-K @Temperature 500 °C | 142 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 22.4 W/m-K @Temperature 600 °C | 155 BTU-in/hr-ft²-°F @Temperature 1110 °F |
Melting Point | 1304 - 1368 °C | 2379 - 2494 °F |
Solidus | 1304 °C | 2379 °F |
Liquidus | 1368 °C | 2494 °F |
|
Processing Properties | Metric | English | Comments |
---|
Annealing Temperature | 1079 °C | 1975 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | <= 0.50 % | <= 0.50 % |
Boron, B | <= 0.0060 % | <= 0.0060 % |
Carbon, C | <= 0.010 % | <= 0.010 % |
Chromium, Cr | 21 % | 21 % |
Cobalt, Co | <= 1.0 % | <= 1.0 % |
Iron, Fe | <= 2.0 % | <= 2.0 % |
Manganese, Mn | <= 0.80 % | <= 0.80 % |
Molybdenum, Mo | 17 % | 17 % |
Nickel, Ni | 57 % | 57 % |
Silicon, Si | <= 0.080 % | <= 0.080 % |
Tungsten, W | <= 1.0 % | <= 1.0 % |
|
Descriptive Properties |
---|
Thermal Diffusivity | 0.0334 cm2/s |
| 0.0362 cm2/s |
| 0.0398 cm2/s |
| 0.0427 cm2/s |
| 0.0454 cm2/s |
| 0.0489 cm2/s |
| 0.0517 cm2/s |