MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

661 Stainless Steel sheet
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 600 Series Stainless Steel

Material Notes: 0.075-3.4 mm thick sheet, heated to 1175°C for 10 minutes, water quenched.

Key Words: UNS R30155, AMS 5376, AMS 5531, AMS 5532, AMS 5585, AMS 5768, AMS 5769, AMS 5794, AMS 5795, ANSI G81.40, ASTM A639, ASTM A567, DIN 1.4971
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.25 g/cc0.298 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 821 MPa119000 psi
 162 MPa
@Temperature 980 °C
23500 psi
@Temperature 1800 °F
 217 MPa
@Temperature 925 °C
31500 psi
@Temperature 1700 °F
 293 MPa
@Temperature 870 °C
42500 psi
@Temperature 1600 °F
 348 MPa
@Temperature 815 °C
50500 psi
@Temperature 1500 °F
 452 MPa
@Temperature 760 °C
65600 psi
@Temperature 1400 °F
 514 MPa
@Temperature 705 °C
74500 psi
@Temperature 1300 °F
 600 MPa
@Temperature 650 °C
87000 psi
@Temperature 1200 °F
 655 MPa
@Temperature 595 °C
95000 psi
@Temperature 1100 °F
 676 MPa
@Temperature 540 °C
98000 psi
@Temperature 1000 °F
 690 MPa
@Temperature 425 °C
100000 psi
@Temperature 797 °F
Tensile Strength, Yield 407 MPa
@Strain 0.2 %
59000 psi
@Strain 0.2 %
 93.1 MPa
@Strain 0.2 %,
Temperature 980 °C
13500 psi
@Strain 0.2 %,
Temperature 1800 °F
 131 MPa
@Strain 0.2 %,
Temperature 925 °C
19000 psi
@Strain 0.2 %,
Temperature 1700 °F
 179 MPa
@Strain 0.2 %,
Temperature 870 °C
26000 psi
@Strain 0.2 %,
Temperature 1600 °F
 210 MPa
@Strain 0.2 %,
Temperature 815 °C
30500 psi
@Strain 0.2 %,
Temperature 1500 °F
 234 MPa
@Strain 0.2 %,
Temperature 760 °C
33900 psi
@Strain 0.2 %,
Temperature 1400 °F
 248 MPa
@Strain 0.2 %,
Temperature 540 °C
36000 psi
@Strain 0.2 %,
Temperature 1000 °F
 255 MPa
@Strain 0.2 %,
Temperature 650 °C
37000 psi
@Strain 0.2 %,
Temperature 1200 °F
 259 MPa
@Strain 0.2 %,
Temperature 705 °C
37600 psi
@Strain 0.2 %,
Temperature 1300 °F
 269 MPa
@Strain 0.2 %,
Temperature 595 °C
39000 psi
@Strain 0.2 %,
Temperature 1100 °F
 272 MPa
@Strain 0.2 %,
Temperature 425 °C
39500 psi
@Strain 0.2 %,
Temperature 797 °F
Elongation at Break 42.5 %42.5 %in 50 mm
 25.5 %
@Temperature 760 °C
25.5 %
@Temperature 1400 °F
in 50 mm
 29.5 %
@Temperature 870 °C
29.5 %
@Temperature 1600 °F
in 50 mm
 31.5 %
@Temperature 705 °C
31.5 %
@Temperature 1300 °F
in 50 mm
 37.5 %
@Temperature 650 °C
37.5 %
@Temperature 1200 °F
in 50 mm
 38 %
@Temperature 815 °C
38 %
@Temperature 1500 °F
in 50 mm
 39.5 %
@Temperature 980 °C
39.5 %
@Temperature 1800 °F
in 50 mm
 40 %
@Temperature 595 °C
40 %
@Temperature 1100 °F
in 50 mm
 42.5 %
@Temperature 425 °C
42.5 %
@Temperature 797 °F
in 50 mm
 42.5 %
@Temperature 540 °C
42.5 %
@Temperature 1000 °F
in 50 mm
 50 %
@Temperature 925 °C
50 %
@Temperature 1700 °F
in 50 mm
Modulus of Elasticity 200 GPa29000 ksiTypical for stainless steel
Machinability 18 %18 %Based on 100% machinability for AISI 1212 steel.
Charpy Impact 81.0 J59.7 ft-lbV-Notch
 87.0 J
@Temperature 760 °C
64.2 ft-lb
@Temperature 1400 °F
V-Notch
 87.0 J
@Temperature 815 °C
64.2 ft-lb
@Temperature 1500 °F
V-Notch
 87.0 J
@Temperature 870 °C
64.2 ft-lb
@Temperature 1600 °F
V-Notch
 88.0 J
@Temperature 705 °C
64.9 ft-lb
@Temperature 1300 °F
V-Notch
 89.0 J
@Temperature 650 °C
65.6 ft-lb
@Temperature 1200 °F
V-Notch
 95.0 J
@Temperature 595 °C
70.1 ft-lb
@Temperature 1100 °F
V-Notch
 108 J
@Temperature 425 °C
79.7 ft-lb
@Temperature 797 °F
V-Notch
 108 J
@Temperature 540 °C
79.7 ft-lb
@Temperature 1000 °F
V-Notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000942 ohm-cm
@Temperature 25.0 °C
0.0000942 ohm-cm
@Temperature 77.0 °F
 0.000100 ohm-cm
@Temperature 200 °C
0.000100 ohm-cm
@Temperature 392 °F
 0.000110 ohm-cm
@Temperature 400 °C
0.000110 ohm-cm
@Temperature 752 °F
 0.000120 ohm-cm
@Temperature 600 °C
0.000120 ohm-cm
@Temperature 1110 °F
 0.000120 ohm-cm
@Temperature 800 °C
0.000120 ohm-cm
@Temperature 1470 °F
 0.000120 ohm-cm
@Temperature 1000 °C
0.000120 ohm-cm
@Temperature 1830 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.0 µm/m-°C
@Temperature 21.0 - 95.0 °C
7.78 µin/in-°F
@Temperature 69.8 - 203 °F
 15.3 µm/m-°C
@Temperature 21.0 - 205 °C
8.50 µin/in-°F
@Temperature 69.8 - 401 °F
 15.3 µm/m-°C
@Temperature 21.0 - 315 °C
8.50 µin/in-°F
@Temperature 69.8 - 599 °F
 16.4 µm/m-°C
@Temperature 21.0 - 540 °C
9.11 µin/in-°F
@Temperature 69.8 - 1000 °F
 17.1 µm/m-°C
@Temperature 21.0 - 650 °C
9.50 µin/in-°F
@Temperature 69.8 - 1200 °F
 17.5 µm/m-°C
@Temperature 21.0 - 760 °C
9.72 µin/in-°F
@Temperature 69.8 - 1400 °F
 17.8 µm/m-°C
@Temperature 21.0 - 870 °C
9.89 µin/in-°F
@Temperature 69.8 - 1600 °F
 18.2 µm/m-°C
@Temperature 21.0 - 980 °C
10.1 µin/in-°F
@Temperature 69.8 - 1800 °F
Specific Heat Capacity 0.435 J/g-°C
@Temperature 21.0 - 100 °C
0.104 BTU/lb-°F
@Temperature 69.8 - 212 °F
Thermal Conductivity  12.3 W/m-K
@Temperature 21.0 °C
85.4 BTU-in/hr-ft²-°F
@Temperature 69.8 °F
 13.1 W/m-K
@Temperature 95.0 °C
90.9 BTU-in/hr-ft²-°F
@Temperature 203 °F
 14.5 W/m-K
@Temperature 205 °C
101 BTU-in/hr-ft²-°F
@Temperature 401 °F
 16.1 W/m-K
@Temperature 315 °C
112 BTU-in/hr-ft²-°F
@Temperature 599 °F
 17.6 W/m-K
@Temperature 425 °C
122 BTU-in/hr-ft²-°F
@Temperature 797 °F
 19.2 W/m-K
@Temperature 540 °C
133 BTU-in/hr-ft²-°F
@Temperature 1000 °F
 20.8 W/m-K
@Temperature 650 °C
144 BTU-in/hr-ft²-°F
@Temperature 1200 °F
Melting Point 1300 - 1355 °C2370 - 2471 °F
Solidus 1300 °C2370 °F
Liquidus 1355 °C2471 °F
Maximum Service Temperature, Air 1040 °C1900 °FContinuous or Intermittent Service
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.080 - 0.16 %0.080 - 0.16 %
Chromium, Cr 20 - 22.5 %20 - 22.5 %
Cobalt, Co 18.5 - 21 %18.5 - 21 %
Iron, Fe 31 %31 %
Manganese, Mn 1.0 - 2.0 %1.0 - 2.0 %
Molybdenum, Mo 2.5 - 3.5 %2.5 - 3.5 %
Nb + Ta 0.75 - 1.25 %0.75 - 1.25 %
Nickel, Ni 19 - 21 %19 - 21 %
Niobium, Nb (Columbium, Cb) 0.50 %0.50 %
Nitrogen, N <= 0.20 %<= 0.20 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %
Tantalum, Ta 0.50 %0.50 %
Tungsten, W 2.0 - 3.0 %2.0 - 3.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
661 Stainless Steel
Overview of materials for T 600 Series Stainless Steel
444 Ferritic Stainless Steel, 18Cr-2Mo (UNS S44400)
301 Stainless Steel
330 Stainless Steel

MQ661J / 13288

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.