MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Atom Adhesives AA-DUCT 2919 Epoxy Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: AA-DUCT 2919 is a non-bleeding, electrically conductive, silver-filled epoxy formulation recommended for electronic bonding, coating, and sealing applications that require good flexibility coupled with good electrical and mechanical properties. This two-part, thixotropic adhesive of refined pure silver and epoxy resin components is free of solvents and copper or carbon additives. It develops resilient, electrically and thermally conducting bonds and coatings between many different and dissimilar materials such as metals, ceramics, glass and plastic insulates. AA-DUCT 2919 cures at room temperature and can be used as a flexible "cold-solder" for heat-sensitive components where hot-soldering is impractical. It also can be used for the assembly and repair of electrical modules, flexible circuits, membrane switches, wave guides, flat cable and high frequency shields.

Appearance: Silver

Cure Type: Heat cure or Room temperature

Mix Ratio by weight: 90:100/Resin:Hardener

Benefits:

  • Free of solvents and copper or carbon additives
  • Coatings between many different and dissimilar materials
Substrates: Metal, Ceramics, Glass and Plastic

Typical Application:

  • Assembly and repair of electrical modules, flexible circuts, membrane switches, wave guides, flat cable and high frequency shields
  • Electronic bonding, coating and sealing applications
  • Can be used as a flexible “cold-solder”

Information provided by Atom Adhesives

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8080
Adhesive Bond Strength  0.621 MPa
@Temperature 25.0 °C,
Time 86400 sec
90.0 psi
@Temperature 77.0 °F,
Time 24.0 hour
Lap shear, alum to alum
 1.17 MPa
@Temperature 65.0 °C,
Time 14400 sec
170 psi
@Temperature 149 °F,
Time 4.00 hour
Lap shear, alum to alum
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 0.00011 ohm-cm0.00011 ohm-cmcured 4 hrs @ 65°C
 0.0016 ohm-cm0.0016 ohm-cmcured 24 hrs @ 25°C
 
Thermal PropertiesMetricEnglishComments
CTE, linear 34.9 µm/m-°C19.4 µin/in-°F
Thermal Conductivity 1.60 W/m-K11.1 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 110 °C230 °F
Minimum Service Temperature, Air -60.0 °C-76.0 °F
Glass Transition Temp, Tg 4.00 °C39.2 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  240 min
@Temperature 65.0 °C
4.00 hour
@Temperature 149 °F
 1440 min
@Temperature 25.0 °C
24.0 hour
@Temperature 77.0 °F
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
Thixotropic Index4.9

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tra-Con Tra-Duct 2956 Low Ion Snap Cure Silver Epoxy Adhesive
Cymat A35620SC 020SS Stabilized Aluminum Foam
CHT Group QSil 7750 Addition Cure, Thermally Conductive Material
Chemours Teflon® PTFE Grade K-10 Fluoropolymer Resin
CENTROPLAST CENTROLYTE ZX Polyethylene terephthalate with lubricant

PATOM045 / 172360

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.