MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Refractory Metals

Niobium, Nb; Soft
Categories: Metal; Nonferrous Metal; Niobium Alloy; Refractory Metal; Pure Element

Material Notes: arc-melted, cold forged, recrystallized for 4 h at 1200ºC

Vendors: PLANSEE SE: Whether it's high temperatures, aggressive chemicals or extreme mechanical loading: PLANSEE supplies a suitable product solution in refractory metals or composite materials. As the world market leader in powder metallurgically produced high performance materials we combine outstanding materials knowledge with profound applications and technology know-how. Visit us at www.plansee.com.

Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.57 g/cc0.310 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 115115
Tensile Strength, Ultimate 330 MPa47900 psi
Tensile Strength, Yield 240 MPa
@Strain 0.2 %
34800 psi
@Strain 0.2 %
Elongation at Break 50 %50 %
Modulus of Elasticity 99.0 GPa14400 ksi
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.268 J/g-°C0.0641 BTU/lb-°F
Thermal Conductivity 54.1 W/m-K375 BTU-in/hr-ft²-°F
Melting Point 2467 °C4473 °F
Boiling Point 4744 °C8571 °F
 
Component Elements PropertiesMetricEnglishComments
Niobium, Nb (Columbium, Cb) 99.9 %99.9 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Niobium, Nb; Unalloyed RG (UNS R04200)
Niobium, Nb (Columbium, Cb); Annealed Sample
Niobium, Nb; High Purity
Goodfellow Niobium 56/Titanium 44 Alloy
Niobium, Nb; Hard

MRNb51 / 100344

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.