MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celanex® 2002-2 PBT, Unfilled
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Celanex 2002-2 is a general purpose, unreinforced polybutylene terephthalate with a good balance of mechanical properties and processability. Celanex 2002-2 ia a medium flow material that contains an internal lubricant.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.31 g/cc1.31 g/ccASTM D792
Density 1.31 g/cc0.0473 lb/in³ISO 1183
Water Absorption 0.090 %
@Temperature 22.8 °C
0.090 %
@Temperature 73.0 °F
24hr immersion; ASTM D570
Linear Mold Shrinkage, Flow 0.018 - 0.020 cm/cm0.018 - 0.020 in/inASTM D955
 0.018 - 0.020 cm/cm0.018 - 0.020 in/inISO 294-4
Melt Flow 20 g/10 min20 g/10 minASTM D1238
 20 g/10 min
@Load 2.16 kg,
Temperature 250 °C
20 g/10 min
@Load 4.76 lb,
Temperature 482 °F
[cm3/10min]; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7878ISO 2039-2
Tensile Strength at Break 55.8 MPa8100 psiASTM D638
 60.0 MPa8700 psi50mm/min; ISO 527-2/1A
Tensile Strength, Yield 55.8 MPa8100 psiASTM D638
 60.0 MPa8700 psi50mm/min; ISO 527-2/1A
 17.9 MPa
@Temperature 121 °C
2600 psi
@Temperature 250 °F
ASTM D638
 24.8 MPa
@Temperature 80.0 °C
3600 psi
@Temperature 176 °F
ASTM D638
 75.8 MPa
@Temperature 0.000 °C
11000 psi
@Temperature 32.0 °F
ASTM D638
 101 MPa
@Temperature -40.0 °C
14600 psi
@Temperature -40.0 °F
ASTM D638
Tensile Stress at Strain 30.0 MPa
@Strain 50 %
4350 psi
@Strain 50 %
ISO 527-2/1A
Elongation at Break >= 50 %>= 50 %
 200 %200 %ASTM D638
Elongation at Yield 3.2 %3.2 %ASTM D638
 4.0 %4.0 %50mm/min; ISO 527-2/1A
 4.4 %
@Temperature 0.000 °C
4.4 %
@Temperature 32.0 °F
ASTM D638
 7.2 %
@Temperature 4.44 °C
7.2 %
@Temperature 40.0 °F
ASTM D638
 17 %
@Temperature 80.0 °C
17 %
@Temperature 176 °F
ASTM D638
 23 %
@Temperature 121 °C
23 %
@Temperature 250 °F
ASTM D638
Tensile Modulus 2.60 GPa377 ksi50mm/min; ISO 527-2/1A
 3.17 GPa460 ksiASTM D638
 0.296 GPa
@Temperature 121 °C
43.0 ksi
@Temperature 250 °F
ASTM D638
 0.469 GPa
@Temperature 80.0 °C
68.0 ksi
@Temperature 176 °F
ASTM D638
 3.10 GPa
@Temperature -40.0 °C
450 ksi
@Temperature -40.0 °F
ASTM D638
Flexural Strength 80.0 MPa11600 psiISO 178
 86.2 MPa12500 psiASTM D790
Flexural Modulus 2.50 GPa363 ksiISO 178
 2.55 GPa370 ksiASTM D790
Izod Impact, Notched 0.481 J/cm0.900 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 5.00 kJ/m²2.38 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched NBNBISO 179/1eU
 19.0 J/cm²
@Temperature -30.0 °C
90.4 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.600 J/cm²2.86 ft-lb/in²ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 60093
Dielectric Constant  3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
ASTM D150
 3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
 4.0
@Frequency 100 Hz
4.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 16.5 kV/mm420 kV/inshort term; ASTM D149
 23.0 kV/mm584 kV/inIEC 60243-1
Dissipation Factor  0.0014
@Frequency 100 Hz
0.0014
@Frequency 100 Hz
IEC 60250
 0.022
@Frequency 1e+6 Hz
0.022
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 127 µm/m-°C70.6 µin/in-°FISO 11359-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1,-2,-3
 225 °C437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 150 °C302 °FISO 75-1, -2
 160 °C320 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C131 °FISO 75-1, -2
 55.0 °C131 °FASTM D648
Vicat Softening Point 190 °C374 °FISO 306
Glass Transition Temp, Tg 60.0 °C140 °FISO 11357-1,-2,-3
Flammability, UL94 HBHB
 HB
@Thickness 0.710 mm
HB
@Thickness 0.0280 in
Oxygen Index 22 %22 %ISO 4589
 
Processing PropertiesMetricEnglishComments
Processing Temperature 65.0 - 93.0 °C149 - 199 °Fcavity
 250 - 260 °C482 - 500 °Fhot runner
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 260 °C464 - 500 °F
Die Temperature 250 - 260 °C482 - 500 °F
Melt Temperature 243 °C469 °FISO 294
 235 - 260 °C455 - 500 °F
Mold Temperature 82.0 °C180 °FISO 294
Injection Velocity 300 mm/sec11.8 in/secISO 294
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4.00 hour4.00 hour
Moisture Content <= 0.020 %<= 0.020 %
Hold Pressure 48.0 MPa6960 psiISO 294
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Celanex® 2002 PBT, Unfilled
Borealis Bormed™ HD810MO Polypropylene Copolymer for Medical Applications
Celanese Hostaform® C 9021 LS POM, UV Resistant
Henkel Loctite® Prism® 7701 Primer for Low Energy Surface Plastics
Celanese Celanex® 2000-3FC PBT, Unfilled

PHCQ017 / 178472

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.