MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Beijing Ranger Chem PBT-201-G0 Flame Retarding FR PBT
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Flame Retardant

Material Notes: Modified PBT Characteristics: Unreinforced grades have abundant strength and flexibility, and have strong characteristics against brittleness. UL-certified slow-burning (94HB) and self-extinguishing grades (94V-0, V-2) exist, and electrical properties exhibited are the highest of any thermoplastic. Low water absorption is exhibited, and excellent electrical properties (CTI and GWIT) are retained over extended periods of usages, even with widely varied temperature and humidity conditions. The surface of molded products is smooth, and a low coefficient of friction is exhibited. As the amount of friction is low, PBT is suitable for use in application requiring friction and wear properties. The material is exceptionally reliable, with small in-use dimensional variation, and superior molding stability and dimensional precision. Long-term chemical resistance is exceptional, and at room temperature, there is almost no degradation in properties after. Both unreinforced and reinforced grades exhibit exceptional flowability, and excellent processability.

Application: VCD drive frames\ Connectors\ Trimmers\ Switch buttons for gas-fired instantaneous water heaters\ Relay blocks\ Driers\ Rectifiers\ Outer handles\ Height sensor cases\ Door mirror stays\ Drive component housings\ Energy saving lamp.

Information provided by Beijing Ranger Chemical Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc
@Temperature 23.0 °C
0.0506 lb/in³
@Temperature 73.4 °F
ASTM D792
Moisture Absorption at Equilibrium 0.10 %
@Temperature 23.0 °C,
Time 86400 sec
0.10 %
@Temperature 73.4 °F,
Time 24.0 hour
ASTM D570
Linear Mold Shrinkage 0.014 - 0.020 cm/cm0.014 - 0.020 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 60.0 MPa8700 psiASTM D638
Flexural Strength 80.0 MPa11600 psiASTM D790
Flexural Modulus 5.00 GPa725 ksiASTM D790
Izod Impact, Notched (ISO) 5.40 kJ/m²2.57 ft-lb/in²ASTM D256
Izod Impact, Unnotched (ISO) 50.0 kJ/m²23.8 ft-lb/in²ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.10e+16 ohm-cm
@Thickness 2.00 mm
1.10e+16 ohm-cm
@Thickness 0.0787 in
ASTM D257
Dielectric Constant 3.0
@Frequency 50 Hz
3.0
@Frequency 50 Hz
ASTM D150
Dielectric Strength 19.0 kV/mm
@Thickness 2.00 mm
483 kV/in
@Thickness 0.0787 in
ASTM D149
Dielectric Loss Index 0.020
@Frequency 50 Hz
0.020
@Frequency 50 Hz
Tangent; ASTM D150
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 180 °C356 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C158 °FASTM D648
Flammability, UL94  V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
 V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 240 °C464 °F
Melt Temperature 225 - 245 °C437 - 473 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
Injection Pressure 40.0 - 100 MPa5800 - 14500 psi
Back Pressure 4.00 - 15.0 MPa580 - 2180 psi
Screw Speed <= 100 rpm<= 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RTP Company RTP 2500 FR-3010 Polycarbonate/ABS Alloy (PC/ABS), Flame Retardant - Bromine/Chlorine Free
Kolon SPESIN® KP212V0BLK Flame Retardant PBT Compound Resin
Ascend Performance Materials Starflam® AFR450B1 PA66, Glass Fiber Reinforced, Flame Retardant, Injection Molding

PRANG075 / 93080

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.