System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Network Polymers Kepital® F20-52
Categories:
Polymer
;
Thermoplastic
;
Acetal (Polyoxymethylene, POM)
;
Acetal Copolymer, Unreinforced
Material Notes:
Description:
Natural Acetal Copolymer, Weather Resistance Grade
Information provided by Network Polymers Inc.
A. Schulman has acquired Network Polymers.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.41
g/cc
1.41
g/cc
ASTM D792
Moisture Absorption at Equilibrium
0.22 %
0.22 %
23°C at 60% RH; ASTM D570
Linear Mold Shrinkage
0.020
cm/cm
0.020
in/in
ASTM D955
Melt Flow
10
g/10 min
@Load 2.16 kg,
Temperature 190 °C
10
g/10 min
@Load 4.76 lb,
Temperature 374 °F
Procedure A Condition E; ASTM D1238
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell M
80
80
ASTM D785
Tensile Strength at Break
56.5
MPa
8200
psi
ASTM D638
Elongation at Break
55 %
55 %
ASTM D638
Flexural Strength
80.7
MPa
11700
psi
ASTM D790
Flexural Modulus
2.452
GPa
355.6
ksi
ASTM D790
Poissons Ratio
0.35
0.35
Shear Strength
55.2
MPa
8000
psi
ASTM D732
Izod Impact, Notched
0.587
J/cm
1.10
ft-lb/in
ASTM D256
Coefficient of Friction
0.13
0.13
Against Steel; Westover or Radial Type
0.15
0.15
Against Aluminum; Westover or Radial Type
0.15
0.15
Against Brass; Westover or Radial Type
0.20
0.20
Against Kepital; Westover or Radial Type
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+14
ohm-cm
1.00e+14
ohm-cm
ASTM D257
Surface Resistance
1.00e+16
ohm
1.00e+16
ohm
ASTM D257
Dielectric Constant
3.7
@Frequency 100 Hz
3.7
@Frequency 100 Hz
ASTM D150
3.7
@Frequency 1e+7 Hz
3.7
@Frequency 1e+7 Hz
ASTM D150
Dissipation Factor
0.0010
@Frequency 100 Hz
0.0010
@Frequency 100 Hz
ASTM D150
0.0070
@Frequency 1e+6 Hz
0.0070
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance
>=
200
sec
>=
200
sec
ASTM D495
Thermal Properties
Metric
English
Comments
CTE, linear
130
µm/m-°C
@Temperature 20.0 °C
72.0
µin/in-°F
@Temperature 68.0 °F
ASTM D696
Melting Point
165
°C
329
°F
10°C/min heating; DSC
Deflection Temperature at 0.46 MPa (66 psi)
158
°C
316
°F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
110
°C
230
°F
ASTM D648
Vicat Softening Point
162
°C
324
°F
0.125 inch bar, 1 Kg; ASTM D1525
Flammability, UL94
HB
@Thickness 0.0790 mm
HB
@Thickness 0.00311 in
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Network Polymers Kepital® F20-03
Network Polymers Kepital® F40-03
Network Polymers Kepital® F10-02
Network Polymers Kepital® F30-03
BASF Ultraform® N2320 006 POM
PDIAM154 / 29992
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.