MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

410 Stainless Steel, tempered at 605°C
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes: 16 mm diameter bar, heated to 980°C for 30 min., oil quenched, 605°C temper for 2 hours, air cooled

Key Words: AFNOR Z 12 C 13, UNI X 12 Cr 13, JIS SUS 410, SS14 2302 (Sweden), B.S. 410 S 21, UNS S41000, AMS 5504, AMS 5505, AMS 5591, AMS 5613, AMS 5776, AMS 5821, ASME SA194 (6), ASME SA240, ASME SA268, ASME SA479, ASTM A176, ASTM A193, ASTM A194, ASTM A240, ASTM A276, ASTM A314, ASTM A473, ASTM A479, ASTM A493, ASTM A511, martensitic, ASTM A580, FED QQ-S-763, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405 (51410), B.S. En. 56 A, B.S. ANC 1 Grade A (U.K), SAE J412 (51410), DIN 1.4006, AFNOR Z 10 C 13, AFNOR Z 10 C 14 (France), ISO 683/13 3
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 300300Converted from Rockwell C hardness
Hardness, Rockwell C 28.528.5before testing
Hardness, Vickers 291291Converted from Rockwell C hardness
Tensile Strength, Ultimate 924 MPa134000 psi
 450 MPa
@Temperature 595 °C
65300 psi
@Temperature 1100 °F
 560 MPa
@Temperature 540 °C
81200 psi
@Temperature 1000 °F
 625 MPa
@Temperature 480 °C
90600 psi
@Temperature 896 °F
 724 MPa
@Temperature 425 °C
105000 psi
@Temperature 797 °F
 772 MPa
@Temperature 315 °C
112000 psi
@Temperature 599 °F
 817 MPa
@Temperature 205 °C
118000 psi
@Temperature 401 °F
Tensile Strength, Yield 807 MPa
@Strain 0.2 %
117000 psi
@Strain 0.2 %
 415 MPa
@Strain 0.2 %,
Temperature 595 °C
60200 psi
@Strain 0.2 %,
Temperature 1100 °F
 525 MPa
@Strain 0.2 %,
Temperature 540 °C
76100 psi
@Strain 0.2 %,
Temperature 1000 °F
 585 MPa
@Strain 0.2 %,
Temperature 480 °C
84800 psi
@Strain 0.2 %,
Temperature 896 °F
 650 MPa
@Strain 0.2 %,
Temperature 425 °C
94300 psi
@Strain 0.2 %,
Temperature 797 °F
 689 MPa
@Strain 0.2 %,
Temperature 315 °C
99900 psi
@Strain 0.2 %,
Temperature 599 °F
 727 MPa
@Strain 0.2 %,
Temperature 205 °C
105000 psi
@Strain 0.2 %,
Temperature 401 °F
Elongation at Break 20 %20 %in 50 mm
 16.5 %
@Temperature 315 °C
16.5 %
@Temperature 599 °F
in 50 mm
 17 %
@Temperature 425 °C
17 %
@Temperature 797 °F
in 50 mm
 17.5 %
@Temperature 205 °C
17.5 %
@Temperature 401 °F
in 50 mm
 18.5 %
@Temperature 480 °C
18.5 %
@Temperature 896 °F
in 50 mm
 22 %
@Temperature 540 °C
22 %
@Temperature 1000 °F
in 50 mm
 25 %
@Temperature 595 °C
25 %
@Temperature 1100 °F
in 50 mm
Reduction of Area 68.5 %68.5 %
 65.5 %
@Temperature 425 °C
65.5 %
@Temperature 797 °F
 67.5 %
@Temperature 315 °C
67.5 %
@Temperature 599 °F
 70.5 %
@Temperature 205 °C
70.5 %
@Temperature 401 °F
 74.5 %
@Temperature 480 °C
74.5 %
@Temperature 896 °F
 82 %
@Temperature 540 °C
82 %
@Temperature 1000 °F
 87 %
@Temperature 595 °C
87 %
@Temperature 1100 °F
Modulus of Elasticity 200 GPa29000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000570 ohm-cm
@Temperature 20.0 °C
0.0000570 ohm-cm
@Temperature 68.0 °F
 0.000108 ohm-cm
@Temperature 650 °C
0.000108 ohm-cm
@Temperature 1200 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.90 µm/m-°C
@Temperature 0.000 - 100 °C
5.50 µin/in-°F
@Temperature 32.0 - 212 °F
 11.0 µm/m-°C
@Temperature 0.000 - 315 °C
6.11 µin/in-°F
@Temperature 32.0 - 599 °F
 11.5 µm/m-°C
@Temperature 0.000 - 540 °C
6.39 µin/in-°F
@Temperature 32.0 - 1000 °F
 11.7 µm/m-°C
@Temperature 0.000 - 650 °C
6.50 µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity  24.9 W/m-K
@Temperature 100 °C
173 BTU-in/hr-ft²-°F
@Temperature 212 °F
 28.7 W/m-K
@Temperature 500 °C
199 BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point 1480 - 1530 °C2700 - 2790 °F
Solidus 1480 °C2700 °F
Liquidus 1530 °C2790 °F
Maximum Service Temperature, Air 705 °C1300 °FContinuous Service
 815 °C1500 °FIntermittent
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.15 %<= 0.15 %
Chromium, Cr 11.5 - 13.5 %11.5 - 13.5 %
Iron, Fe 84.3 - 88.5 %84.3 - 88.5 %as balance
Manganese, Mn <= 1.0 %<= 1.0 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
410 Stainless Steel
410 Stainless Steel, tempered at 233°C
410 Stainless Steel, tempered at 343°C
410 Stainless Steel, tempered at 453°C
410 Stainless Steel, tempered at 540°C (1000°F)

MQ410AZ / 12974

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.