MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI E4340 H Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: AISI E4340H has a favorable response to heat treatment (usually oil quenching followed by tempering) and exhibits a good combination of ductility and strength when treated thusly. Uses include piston pins, bearings, ordnance, gears, dies, and pressure vessels.

Key Words: AISI E4340H; alloy steels, UNS H43406, ASTM A304, SAE J1268, DIN 1.6562
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 555555Converted from Vickers hardness.
 572
@Temperature -78.0 °C
572
@Temperature -108 °F
Converted from Vickers hardness
 666
@Temperature -195 °C
666
@Temperature -319 °F
Converted from Vickers hardness
 851
@Temperature -255 °C
851
@Temperature -427 °F
Converted from Vickers hardness
Hardness, Vickers 531531
 548
@Temperature -78.0 °C
548
@Temperature -108 °F
 639
@Temperature -195 °C
639
@Temperature -319 °F
 818
@Temperature -255 °C
818
@Temperature -427 °F
Tensile Strength, Ultimate 1855 MPa269000 psi
 2020 MPa
@Temperature -78.0 °C
293000 psi
@Temperature -108 °F
 2200 MPa
@Temperature -195 °C
319000 psi
@Temperature -319 °F
 2290 MPa
@Temperature -255 °C
332000 psi
@Temperature -427 °F
Tensile Strength, Yield 1550 MPa225000 psi
 1915 MPa
@Temperature -195 °C
277700 psi
@Temperature -319 °F
 1935 MPa
@Temperature -78.0 °C
280600 psi
@Temperature -108 °F
Elongation at Break 12 %12 %in 50 mm
 0.60 %
@Temperature -255 °C
0.60 %
@Temperature -427 °F
in 50 mm
 10 %
@Temperature -195 °C
10 %
@Temperature -319 °F
in 50 mm
 12 %
@Temperature -78.0 °C
12 %
@Temperature -108 °F
in 50 mm
Reduction of Area 40 %40 %
 0.20 %
@Temperature -255 °C
0.20 %
@Temperature -427 °F
 24 %
@Temperature -195 °C
24 %
@Temperature -319 °F
 40 %
@Temperature -78.0 °C
40 %
@Temperature -108 °F
Modulus of Elasticity 196 GPa28400 ksi
 210 GPa
@Temperature -255 °C
30500 ksi
@Temperature -427 °F
 211 GPa
@Temperature -195 °C
30600 ksi
@Temperature -319 °F
 211 GPa
@Temperature -78.0 °C
30600 ksi
@Temperature -108 °F
Bulk Modulus 160 GPa23200 ksiTypical for steel.
Poissons Ratio 0.300.30Calculated
Machinability 50 %50 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 75.0 GPa10900 ksiEstimated from elastic modulus
 81.0 GPa
@Temperature -255 °C
11700 ksi
@Temperature -427 °F
Estimated from elastic modulus
 81.0 GPa
@Temperature -195 °C
11700 ksi
@Temperature -319 °F
Estimated from elastic modulus
 81.0 GPa
@Temperature -78.0 °C
11700 ksi
@Temperature -108 °F
Estimated from elastic modulus
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000248 ohm-cm
@Temperature 20.0 °C
0.0000248 ohm-cm
@Temperature 68.0 °F
 0.0000298 ohm-cm
@Temperature 100 °C
0.0000298 ohm-cm
@Temperature 212 °F
 0.0000552 ohm-cm
@Temperature 400 °C
0.0000552 ohm-cm
@Temperature 752 °F
 0.0000797 ohm-cm
@Temperature 600 °C
0.0000797 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.3 µm/m-°C
@Temperature -70.0 - 20.0 °C
6.28 µin/in-°F
@Temperature -94.0 - 68.0 °F
Austenitized 870°C (1600°F), 545°C (1010°F) temper for 2 hrs.
 12.4 µm/m-°C
@Temperature 21.0 - 260 °C
6.89 µin/in-°F
@Temperature 69.8 - 500 °F
Austenitized 870°C (1600°F), 545°C (1010°F) temper for 2 hrs.
 13.7 µm/m-°C
@Temperature 500 °C
7.61 µin/in-°F
@Temperature 932 °F
austenitized at 870°C (1600°F), 545°C (1010°F) temper for 2 hours
Specific Heat Capacity 0.475 J/g-°C0.114 BTU/lb-°FTypical 4000 series steel
Thermal Conductivity 44.5 W/m-K309 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.37 - 0.44 %0.37 - 0.44 %
Chromium, Cr 0.65 - 0.95 %0.65 - 0.95 %
Iron, Fe 95.015 - 96.48 %95.015 - 96.48 %As remainder
Manganese, Mn 0.60 - 0.95 %0.60 - 0.95 %
Molybdenum, Mo 0.20 - 0.30 %0.20 - 0.30 %
Nickel, Ni 1.55 - 2.0 %1.55 - 2.0 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si 0.15 - 0.30 %0.15 - 0.30 %
Sulfur, S <= 0.020 %<= 0.020 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI E4340 H Steel, normalized, oil quenched and tempered
AISI E4340 H Steel, normalized, oil quenched and tempered, nitrided for 50 hrs
AISI E4340 H Steel, oil quenched 800°C (1470°F), 650°C (1200°F) temper, 100 mm (4 in.) round
AISI E4340 H Steel, oil quenched 845°C, 650°C (1200°F) temper
AISI E4340 H Steel, normalized, oil quenched and tempered, nitrided for 48 hrs

M434EU / 7838

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.