MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Elkem (Bluestar Silicones) SILBIONE® LSR 4330 Liquid Silicone Rubber
Categories: Polymer; Thermoset; Silicone; Silicone Rubber; Liquid Silicone Rubber (LSR)

Material Notes: Description: SILBIONE® LSR 4330 is a developmental 30 durometer, healthcare grade liquid silicone rubber designed for producing high clarity, high strength molded parts.

Applications:

  • General molded parts
  • Medical applications for <30 day implantation
  • Infant care; baby bottle nipples, pacifiers, sippy cup valves
  • Food contact applications
Features:
  • Superior clarity
  • High tear strength
  • Excellent mold release for shorter cycle times
  • Rapid cure at elevated temperature
  • No post cure is needed

Information provided by Bluestar Silicones

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.11 g/cc1.11 g/ccTP 013
Viscosity  270000 cP
@Shear Rate 10 1/s
270000 cP
@Shear Rate 10 1/s
 550000 cP
@Shear Rate 1 1/s
550000 cP
@Shear Rate 1 1/s
Storage Temperature 24.0 °C75.2 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 3030Press Cured, 5 min, 177°C; ASTM D2240
 31314 hr post cure @ 200°C; ASTM D2240
Tensile Strength 9.31 MPa1350 psi4 hr post cure @ 200°C; ASTM D412
 9.65 MPa1400 psiPress Cured, 5 min, 177°C; ASTM D412
Elongation at Break 750 %750 %4 hr post cure @ 200°C; ASTM D412
 790 %790 %Press Cured, 5 min, 177°C; ASTM D412
100% Modulus  1.31 MPa
@Strain 100 %
190 psi
@Strain 100 %
Press Cured, 5 min, 177°C; ASTM D412
 1.38 MPa
@Strain 100 %
200 psi
@Strain 100 %
4 hr post cure @ 200°C; ASTM D412
Tear Strength 34.2 kN/m195 pliPress Cured, 5 min, 177°C; ASTM D624, Die B
 35.9 kN/m205 pli4 hr post cure @ 200°C; ASTM D624, Die B
Compression Set 10 %10 %4 hr post cure @ 200°C; ASTM D395B
 35 %35 %Press Cured, 5 min, 177°C; ASTM D395B
 
Processing PropertiesMetricEnglishComments
Extrusion Rate 105 g/min105 g/minTP 001
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
AppearanceTP 038
Resiliency (%)604 hr post cure @ 200°C, ASTM D2632
 62Press Cured, 5 min, 177°C, ASTM D2632

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient Synprene® IT 38-074 Thermoplastic Elastomer - SBC
Dow Silastic® NPC 9300-40 LSR Non-Post-Cure Liquid Silicone Rubber
Dow C6-530 LIQUID SILICONE RUBBER KIT
Elkem (Bluestar Silicones) SILBIONE® LSR 4325 Liquid Silicone Rubber
Dow Silastic® NPC 9310-50 LSR Non-Post-Cure Liquid Silicone Rubber

PBLUST069 / 191045

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.