MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LATI Laramid G/45 PPA, 45% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 50% Glass Fiber Reinforced

Material Notes: Semi-aromatic polyamide (PPA) based compound. Glass fibers. Very good thermal properties. Good chemical resistance. Low moisture absorption.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Information provided by Lati Industria Termoplastici S.p.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.55 g/cc0.0560 lb/in³
Linear Mold Shrinkage, Flow 0.0025 - 0.0050 cm/cm0.0025 - 0.0050 in/in
Linear Mold Shrinkage, Transverse 0.0060 - 0.0090 cm/cm0.0060 - 0.0090 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  95.0 MPa
@Temperature 150 °C
13800 psi
@Temperature 302 °F
 150 MPa
@Temperature 120 °C
21800 psi
@Temperature 248 °F
 170 MPa
@Temperature 90.0 °C
24700 psi
@Temperature 194 °F
 195 MPa
@Temperature 60.0 °C
28300 psi
@Temperature 140 °F
 245 MPa
@Temperature 23.0 °C
35500 psi
@Temperature 73.4 °F
Elongation at Break  2.2 %
@Temperature 23.0 °C
2.2 %
@Temperature 73.4 °F
 2.4 %
@Temperature 60.0 °C
2.4 %
@Temperature 140 °F
 2.5 %
@Temperature 90.0 °C
2.5 %
@Temperature 194 °F
 4.0 %
@Temperature 120 °C
4.0 %
@Temperature 248 °F
 6.8 %
@Temperature 150 °C
6.8 %
@Temperature 302 °F
Tensile Modulus  5.80 GPa
@Temperature 150 °C
841 ksi
@Temperature 302 °F
 10.5 GPa
@Temperature 120 °C
1520 ksi
@Temperature 248 °F
 12.0 GPa
@Temperature 90.0 °C
1740 ksi
@Temperature 194 °F
 14.0 GPa
@Temperature 60.0 °C
2030 ksi
@Temperature 140 °F
 17.5 GPa
@Temperature 23.0 °C
2540 ksi
@Temperature 73.4 °F
Charpy Impact Unnotched 8.50 J/cm²40.4 ft-lb/in²
Charpy Impact, Notched 1.00 J/cm²4.76 ft-lb/in²
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 150 °C302 °F
Deflection Temperature at 0.46 MPa (66 psi) 290 °C554 °F
Deflection Temperature at 1.8 MPa (264 psi) 280 °C536 °F
Vicat Softening Point 275 °C
@Load 5.00 kg
527 °F
@Load 11.0 lb
 
Processing PropertiesMetricEnglishComments
Melt Temperature 310 - 340 °C590 - 644 °F
Mold Temperature 150 - 170 °C302 - 338 °F
Drying Temperature 120 - 130 °C
@Time 10800 sec
248 - 266 °F
@Time 3.00 hour
 
Descriptive Properties
ISO Shrinkage - Pressure60 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Techmer ES HiFill® PPA GF45 HS L X 45% Glass Filled
Eurotec® Tecomid® NT40 GR50 NL HS PPA, 50% glass fiber reinforced, heat stabilized, natural
E-Polymers SEPAZ® V240A 40% Glass Fiber Reinforced PPA
DuPont Mobility and Materials Zytel® HTN 55G55LWSF BK752A Polyphthalamide (PPA)
DuPont Mobility and Materials Zytel® HTN 54G35HSLR BKB336 Polyphthalamide (PPA)

PLATH9624 / 177320

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.