MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

CeramTec AT 79 Alumina, 99.6%
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Aluminas exhibit good mechanical properties such as hardness, compressive and tensile strength, and elastic modulus. They perform well at elevated temperatures.

Key Words: Al2O3, aluminum oxide
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 3.95 g/cc0.143 lb/in³DIN EN 623-2
Water Absorption 0.00 %0.00 %Open Porosity; DIN EN 623-2
Permeability 0.000.00%, Gas
Weibull Modulus 1414DINV ENV 843-5
 
Mechanical PropertiesMetricEnglishComments
Vickers Microhardness 21102110HV1; DINV ENV 843-4
Tensile Modulus 390 GPa56600 ksiYoung's; DINV ENV 843-2
Flexural Strength 470 MPa68200 psiDIN EN 843-1
Compressive Strength 4000 MPa580000 psiDIN 51067T1
Poissons Ratio 0.230.23DINV ENV 843-2
Fracture Toughness 4.00 MPa-m½3.64 ksi-in½KIC (SEVNB); DIN CEN/TS 14425-1
Shear Modulus 159 GPa23100 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  5.00e+8 ohm-cm
@Temperature 400 °C
5.00e+8 ohm-cm
@Temperature 752 °F
IEC 672-1
 5.00e+14 ohm-cm
@Temperature 20.0 °C
5.00e+14 ohm-cm
@Temperature 68.0 °F
IEC 672-1
Dielectric Constant 9.0
@Frequency 1e+6 Hz
9.0
@Frequency 1e+6 Hz
IEC 672-1
Dielectric Strength 18.0 kV/mm457 kV/inIEC 672-1
Dielectric Loss Index 0.0050
@Frequency 9.00e+9 Hz
0.0050
@Frequency 9.00e+9 Hz
IEC 672-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.50 µm/m-°C
@Temperature 20.0 - 100 °C
4.17 µin/in-°F
@Temperature 68.0 - 212 °F
DIN EN 821-1
Specific Heat Capacity 0.900 J/g-°C0.215 BTU/lb-°FDINV ENV 821-3
Thermal Conductivity 30.0 W/m-K208 BTU-in/hr-ft²-°FDIN EN 821-2
Maximum Service Temperature, Air 1500 °C2730 °F
Maximum Service Temperature, Inert 1500 °C2730 °F
 
Component Elements PropertiesMetricEnglishComments
Al2O3 99.6 %99.6 %
 
Descriptive Properties
Ra = Arithmetic Mean Roughness Value (µm)<0.1
Thermal Shock Resistance R1 (K)127calculated; R1 = [σs (1-µ)] / (α·E)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CeramTec RK 87 Alumina, 99.8%
CeramTec V 38 Alumina, 96.0% Al2O3-SiO2
CeramTec B 601 Alumina, 98.5%
CeramTec 771 94% Alumina (Al2O3)
CeramTec B 40 Alumina, 99.1%

CCERA905 / 107505

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.