Physical Properties | Metric | English | Comments |
---|
Density | 7.87 g/cc | 0.284 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 311 | 311 |
Hardness, Knoop | 338 | 338 |
Hardness, Rockwell B | 99 | 99 |
Hardness, Rockwell C | 34 | 34 |
Hardness, Vickers | 329 | 329 |
Tensile Strength, Ultimate | 1080 MPa | 157000 psi |
Tensile Strength, Yield | 620 MPa | 89900 psi |
Elongation at Break | 11.5 % | 11.5 % |
Reduction of Area | 24.4 % | 24.4 % |
Modulus of Elasticity | 200 GPa | 29000 ksi |
Bulk Modulus | 160 GPa | 23200 ksi |
Poissons Ratio | 0.29 | 0.29 |
Shear Modulus | 80.0 GPa | 11600 ksi |
Izod Impact | 7.00 J | 5.16 ft-lb |
| 7.00 J | 5.16 ft-lb |
| 7.00 J | 5.16 ft-lb |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000180 ohm-cm @Temperature 20.0 °C | 0.0000180 ohm-cm @Temperature 68.0 °F |
| 0.0000232 ohm-cm @Temperature 100 °C | 0.0000232 ohm-cm @Temperature 212 °F |
| 0.0000308 ohm-cm @Temperature 200 °C | 0.0000308 ohm-cm @Temperature 392 °F |
| 0.0000505 ohm-cm @Temperature 400 °C | 0.0000505 ohm-cm @Temperature 752 °F |
| 0.0000772 ohm-cm @Temperature 600 °C | 0.0000772 ohm-cm @Temperature 1110 °F |
| 0.0000935 ohm-cm @Temperature 700 °C | 0.0000935 ohm-cm @Temperature 1290 °F |
| 0.0001129 ohm-cm @Temperature 800 °C | 0.0001129 ohm-cm @Temperature 1470 °F |
| 0.0001164 ohm-cm @Temperature 900 °C | 0.0001164 ohm-cm @Temperature 1650 °F |
| 0.0001246 ohm-cm @Temperature 1250 °C | 0.0001246 ohm-cm @Temperature 2280 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 11.0 µm/m-°C @Temperature 0.000 - 100 °C | 6.11 µin/in-°F @Temperature 32.0 - 212 °F |
| 11.5 µm/m-°C @Temperature 0.000 - 200 °C | 6.39 µin/in-°F @Temperature 32.0 - 392 °F |
| 12.2 µm/m-°C @Temperature 0.000 - 300 °C | 6.78 µin/in-°F @Temperature 32.0 - 572 °F |
| 13.1 µm/m-°C @Temperature 0.000 - 400 °C | 7.28 µin/in-°F @Temperature 32.0 - 752 °F |
| 13.7 µm/m-°C @Temperature 0.000 - 500 °C | 7.61 µin/in-°F @Temperature 32.0 - 932 °F |
| 14.0 µm/m-°C @Temperature 0.000 - 600 °C | 7.78 µin/in-°F @Temperature 32.0 - 1110 °F |
| 14.6 µm/m-°C @Temperature 0.000 - 700 °C | 8.11 µin/in-°F @Temperature 32.0 - 1290 °F |
Specific Heat Capacity | 0.490 J/g-°C @Temperature >=100 °C | 0.117 BTU/lb-°F @Temperature >=212 °F |
| 0.531 J/g-°C @Temperature 150 - 200 °C | 0.127 BTU/lb-°F @Temperature 302 - 392 °F |
| 0.548 J/g-°C @Temperature 200 - 250 °C | 0.131 BTU/lb-°F @Temperature 392 - 482 °F |
| 0.565 J/g-°C @Temperature 250 - 300 °C | 0.135 BTU/lb-°F @Temperature 482 - 572 °F |
| 0.586 J/g-°C @Temperature 300 - 350 °C | 0.140 BTU/lb-°F @Temperature 572 - 662 °F |
| 0.607 J/g-°C @Temperature 350 - 400 °C | 0.145 BTU/lb-°F @Temperature 662 - 752 °F |
| 0.615 J/g-°C @Temperature 750 - 800 °C | 0.147 BTU/lb-°F @Temperature 1380 - 1470 °F |
| 0.670 J/g-°C @Temperature 450 - 500 °C | 0.160 BTU/lb-°F @Temperature 842 - 932 °F |
| 0.712 J/g-°C @Temperature 550 - 600 °C | 0.170 BTU/lb-°F @Temperature 1020 - 1110 °F |
| 0.770 J/g-°C @Temperature 650 - 700 °C | 0.184 BTU/lb-°F @Temperature 1200 - 1290 °F |
| 2.08 J/g-°C @Temperature 700 - 750 °C | 0.497 BTU/lb-°F @Temperature 1290 - 1380 °F |
Thermal Conductivity | 24.4 W/m-K @Temperature 800 °C | 169 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 26.8 W/m-K @Temperature 1000 °C | 186 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 30.1 W/m-K @Temperature 700 °C | 209 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 30.1 W/m-K @Temperature 1200 °C | 209 BTU-in/hr-ft²-°F @Temperature 2190 °F |
| 32.7 W/m-K @Temperature 600 °C | 227 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 35.1 W/m-K @Temperature 500 °C | 244 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 38.1 W/m-K @Temperature 400 °C | 264 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 41.3 W/m-K @Temperature 300 °C | 287 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 45.2 W/m-K @Temperature 200 °C | 314 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 47.7 W/m-K @Temperature 0.000 °C | 331 BTU-in/hr-ft²-°F @Temperature 32.0 °F |
| 48.1 W/m-K @Temperature 100 °C | 334 BTU-in/hr-ft²-°F @Temperature 212 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.75 - 0.88 % | 0.75 - 0.88 % |
Iron, Fe | 98.13 - 98.65 % | 98.13 - 98.65 % |
Manganese, Mn | 0.60 - 0.90 % | 0.60 - 0.90 % |
Phosphorus, P | <= 0.040 % | <= 0.040 % |
Sulfur, S | <= 0.050 % | <= 0.050 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.