MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Cosmic Plastics K77/6220F Short Glass Fiber Filled Diallyl Iso-Phthalate Molding Compound  (discontinued **)
Categories: Polymer; Thermoset; Diallyl Phthalate (DAP); Diallyl Phthalate (DAP) Molding Compound, Short Glass Fiber Filled

Material Notes: Description: Cosmic K77 / 6220F is a short glass fiber filled, flame retardant premium diallyl iso-phthalate molding compound which is supplied in a granular form. It pours easily, can be preformed, and molds easily in standard compression, transfer or injection equipment.

Features: K77 / 6220F has good impact strength, excellent electrical properties and very high heat service properties.

Applications: The high strength of this material makes it ideal for switches, terminals, housings, structural parts and insulators.

Information provided by Cosmic Plastics Inc

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.78 g/cc1.78 g/cc
Bulk Factor 2.52.5
Water Absorption 0.25 %
@Temperature 50.0 °C,
Time 173000 sec
0.25 %
@Temperature 122 °F,
Time 48.0 hour
Linear Mold Shrinkage 0.0010 - 0.0040 cm/cm0.0010 - 0.0040 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 41.4 - 68.9 MPa6000 - 10000 psi
Flexural Strength 89.6 - 103 MPa13000 - 15000 psi
Compressive Strength 165 - 179 MPa24000 - 26000 psi
Izod Impact, Notched 0.267 - 0.667 J/cm0.500 - 1.25 ft-lb/in
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cm
 1.00e+10 ohm-cm
@Temperature 70.0 °C,
Time 2.59e+6 sec
1.00e+10 ohm-cm
@Temperature 158 °F,
Time 720 hour
100% RH
Surface Resistance >= 1.00e+16 ohm>= 1.00e+16 ohm
 1.00e+10 ohm
@Temperature 70.0 °C,
Time 2.59e+6 sec
1.00e+10 ohm
@Temperature 158 °F,
Time 720 hour
100% RH
Dielectric Constant  3.9
@Frequency 1e+6 Hz
3.9
@Frequency 1e+6 Hz
Dry
 4.2
@Frequency 1000 Hz
4.2
@Frequency 1000 Hz
Dry
 4.2
@Frequency 1e+6 Hz
4.2
@Frequency 1e+6 Hz
Wet
 4.3
@Frequency 1000 Hz
4.3
@Frequency 1000 Hz
Wet
Dielectric Strength 15.7 kV/mm400 kV/inDry, step by step
 15.7 kV/mm400 kV/inWet, step by step
Dielectric Breakdown 60 V60 VWet, step by step
 64 V64 VDry, step by step
Dissipation Factor  0.0070
@Frequency 1000 Hz
0.0070
@Frequency 1000 Hz
Dry
 0.010
@Frequency 1000 Hz
0.010
@Frequency 1000 Hz
Wet
 0.014
@Frequency 1e+6 Hz
0.014
@Frequency 1e+6 Hz
Dry
 0.015
@Frequency 1e+6 Hz
0.015
@Frequency 1e+6 Hz
Wet
Arc Resistance 180 sec180 sec
 
Thermal PropertiesMetricEnglishComments
CTE, linear 15.0 µm/m-°C
@Temperature -40.0 - 100 °C
8.33 µin/in-°F
@Temperature -40.0 - 212 °F
Heat Distortion Temperature 260 °C500 °F
Flammability, UL94 V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in
 
Processing PropertiesMetricEnglishComments
Mold Temperature 135 - 170 °C275 - 338 °F
 
Descriptive Properties
Dimensional Stability<0.01%
MIL-M-14SDG-FASTM D5948-96
 SIG-FASTM D5948-96
Molding Pressure500-8000 psi

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
PSM Industries Pacific Sintered Metals FCC-214-S High Carbon Copper Steel Powdered Metal (MPIF FC-0208-50)
Cosmic Plastics D33 Short Glass Fiber Filled Diallyl Iso-Phthalate Molding Compound
Cosmic Plastics D69/6130 Long Glass Fiber Filled Diallyl Iso-Phthalate Molding Compound
PSM Industries Pacific Sintered Metals FCC-200-P High Carbon Copper Steel Powdered Metal (MPIF FC-0505-40)
PSM Industries Pacific Sintered Metals FCC-214-S(HT) High Carbon Copper Steel Powdered Metal (MPIF FC-0208-80HT)

PCOSM015 / 190797

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.