Physical Properties | Metric | English | Comments |
---|
Density | 9.13 g/cc | 0.330 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 930 MPa | 135000 psi |
Tensile Strength, Yield | 460 MPa @Strain 0.2 % | 66700 psi @Strain 0.2 % |
Elongation at Break | 48.7 % | 48.7 % |
Modulus of Elasticity | 225 GPa | 32600 ksi |
| 146 GPa @Temperature 1000 °C | 21200 ksi @Temperature 1830 °F |
| 154 GPa @Temperature 900 °C | 22300 ksi @Temperature 1650 °F |
| 163 GPa @Temperature 800 °C | 23600 ksi @Temperature 1470 °F |
| 174 GPa @Temperature 700 °C | 25200 ksi @Temperature 1290 °F |
| 181 GPa @Temperature 600 °C | 26300 ksi @Temperature 1110 °F |
| 188 GPa @Temperature 500 °C | 27300 ksi @Temperature 932 °F |
| 197 GPa @Temperature 400 °C | 28600 ksi @Temperature 752 °F |
| 204 GPa @Temperature 300 °C | 29600 ksi @Temperature 572 °F |
| 214 GPa @Temperature 200 °C | 31000 ksi @Temperature 392 °F |
| 222 GPa @Temperature 100 °C | 32200 ksi @Temperature 212 °F |
Charpy Impact | 262 J | 193 ft-lb |
| 144 J @Temperature 980 °C | 106 ft-lb @Temperature 1800 °F |
| 148 J @Temperature -196 °C | 109 ft-lb @Temperature -321 °F |
| 163 J @Temperature 870 °C | 120 ft-lb @Temperature 1600 °F |
| 182 J @Temperature -138 °C | 134 ft-lb @Temperature -216 °F |
| 194 J @Temperature 760 °C | 143 ft-lb @Temperature 1400 °F |
| 212 J @Temperature -78.0 °C | 156 ft-lb @Temperature -108 °F |
| 230 J @Temperature 650 °C | 170 ft-lb @Temperature 1200 °F |
| 243 J @Temperature -29.0 °C | 179 ft-lb @Temperature -20.2 °F |
| 273 J @Temperature 540 °C | 201 ft-lb @Temperature 1000 °F |
| 297 J @Temperature 260 °C | 219 ft-lb @Temperature 500 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000886 ohm-cm | 0.0000886 ohm-cm |
| 0.0000950 ohm-cm @Temperature 1000 °C | 0.0000950 ohm-cm @Temperature 1830 °F |
| 0.0001011 ohm-cm @Temperature 900 °C | 0.0001011 ohm-cm @Temperature 1650 °F |
| 0.0001066 ohm-cm @Temperature 700 °C | 0.0001066 ohm-cm @Temperature 1290 °F |
| 0.0001078 ohm-cm @Temperature 800 °C | 0.0001078 ohm-cm @Temperature 1470 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.3 µm/m-°C @Temperature 25.0 - 100 °C | 6.83 µin/in-°F @Temperature 77.0 - 212 °F |
| 12.9 µm/m-°C @Temperature 25.0 - 200 °C | 7.17 µin/in-°F @Temperature 77.0 - 392 °F |
| 13.6 µm/m-°C @Temperature 25.0 - 300 °C | 7.56 µin/in-°F @Temperature 77.0 - 572 °F |
| 14.3 µm/m-°C @Temperature 25.0 - 500 °C | 7.94 µin/in-°F @Temperature 77.0 - 932 °F |
| 14.3 µm/m-°C @Temperature 25.0 - 400 °C | 7.94 µin/in-°F @Temperature 77.0 - 752 °F |
| 14.6 µm/m-°C @Temperature 25.0 - 600 °C | 8.11 µin/in-°F @Temperature 77.0 - 1110 °F |
| 15.1 µm/m-°C @Temperature 25.0 - 700 °C | 8.39 µin/in-°F @Temperature 77.0 - 1290 °F |
| 15.8 µm/m-°C @Temperature 25.0 - 800 °C | 8.78 µin/in-°F @Temperature 77.0 - 1470 °F |
| 16.5 µm/m-°C @Temperature 25.0 - 900 °C | 9.17 µin/in-°F @Temperature 77.0 - 1650 °F |
| 17.0 µm/m-°C @Temperature 25.0 - 1000 °C | 9.44 µin/in-°F @Temperature 77.0 - 1830 °F |
Thermal Conductivity | 9.40 W/m-K | 65.2 BTU-in/hr-ft²-°F |
| 10.9 W/m-K @Temperature 100 °C | 75.6 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 12.9 W/m-K @Temperature 200 °C | 89.5 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 14.8 W/m-K @Temperature 300 °C | 103 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 16.8 W/m-K @Temperature 400 °C | 117 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 18.7 W/m-K @Temperature 500 °C | 130 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 20.7 W/m-K @Temperature 600 °C | 144 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 22.6 W/m-K @Temperature 700 °C | 157 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 24.7 W/m-K @Temperature 800 °C | 171 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 26.7 W/m-K @Temperature 900 °C | 185 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 29.2 W/m-K @Temperature 1000 °C | 203 BTU-in/hr-ft²-°F @Temperature 1830 °F |
Melting Point | 1330 - 1410 °C | 2430 - 2570 °F |
Solidus | 1330 °C | 2430 °F |
Liquidus | 1410 °C | 2570 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.10 % | 0.10 % |
Chromium, Cr | 20 % | 20 % |
Cobalt, Co | 51 % | 51 % |
Iron, Fe | <= 3.0 % | <= 3.0 % |
Manganese, Mn | 1.5 % | 1.5 % |
Nickel, Ni | 10 % | 10 % |
Silicon, Si | <= 0.40 % | <= 0.40 % |
Tungsten, W | 15 % | 15 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.