MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Domo TECHNYL® C 52G1 V20 GREY R7035 PA 6 20% Glass Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled

Material Notes: Description: TECHNYL C 52G1 V20 GREY R7035 is a 20% glass fiber reinforced, halogen and red phosphorus free flame retarded grade based on polyamide 6, for injection molding. This product is available in grey color.

Key Properties: GWFI 960°C; Excellent electrical performance; Easy processing; Good surface aspect

Benefits: This grade is Halogen and Red Phosphorous free fire resistant flame retardant grade with excellent molding and electrical performance.

Applications: It is particularly suitable for equipment requiring robust glow-wire resistance such as for MCB housings, contactors and switches and sockets.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.32 g/cc0.0477 lb/in³ISO 1183/A
Water Absorption 1.1 %
@Time 86400 sec
1.1 %
@Time 24.0 hour
ISO 62
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 92.0 MPa13300 psiISO 527 Type 1A
Elongation at Break 2.9 %2.9 %ISO 527 Type 1A
Tensile Modulus 6.70 GPa972 ksiISO 527 Type 1A
Charpy Impact Unnotched 3.90 J/cm²18.6 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched  0.310 J/cm²
@Temperature -30.0 °C
1.48 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.320 J/cm²
@Temperature 23.0 °C
1.52 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 31.0 kV/mm787 kV/inIEC 60243
Comparative Tracking Index 450 V450 VSol A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 222 °C432 °FISO 11357
Deflection Temperature at 0.46 MPa (66 psi) 210 °C410 °FISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi) 170 °C338 °FISO 75/Af
Flammability, UL94  V-2
@Thickness 0.800 mm
V-2
@Thickness 0.0315 in
ISO 1210
 V-2
@Thickness 1.60 mm
V-2
@Thickness 0.0630 in
ISO 1210
 V-2
@Thickness 3.20 mm
V-2
@Thickness 0.126 in
ISO 1210
Oxygen Index 29 %29 %ISO 4589
Glow Wire Test  700 °C
@Thickness 1.60 mm
1290 °F
@Thickness 0.0630 in
Ignition Temp; ISO 60695-2-13
 725 °C
@Thickness 0.800 mm
1340 °F
@Thickness 0.0315 in
Ignition Temp; ISO 60695-2-13
 960 °C
@Thickness 1.60 mm
1760 °F
@Thickness 0.0630 in
Flammability Index; ISO 60695-2-12
 960 °C
@Thickness 3.20 mm
1760 °F
@Thickness 0.126 in
Flammability Index; ISO 60695-2-12
 
Processing PropertiesMetricEnglishComments
Processing Temperature 235 - 240 °C455 - 464 °FCompression zone
 240 - 250 °C464 - 482 °FMixing zone
Feed Temperature 230 - 235 °C446 - 455 °F
Mold Temperature 60.0 - 90.0 °C140 - 194 °F
Drying Temperature 80.0 °C176 °F
Moisture Content <= 0.20 %<= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Domo TECHNYL® C 52G1 V20 GREY R7035 PA 6 20% Glass Reinforced, Conditioned
Celanese Zytel® 70K20HSL BK284 PA66-RF20
Domo TECHNYL® C 52G1 V25 Grey R7035 (XC 1329/A) PA6, DRY
Domo Technyl® A 246M Nylon 66, Impact Grade, EH0
Domo TECHNYL® A 218 V20 Black 21N PA66, 20% glass fiber, DRY

PSOLVAY865 / 218593

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.