MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

INEOS Styrolution Lustran® LGM Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Lustran® LGM is a low-gloss, easy-flow grade of ABS (Acrylonitrile Butadiene Styrene). This general-purpose injection molding grade offers an excellent balance of rigidity, impact strength, and abuse resistance. Easy flow, Low gloss, Abuse resistant, Balance of rigidity and impact strength, UL 94 HB rated. Applications: Power tool housings, Lawn and garden, Business machines, Keyboard and keys

Information provided by Styrolution.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ASTM D 792
Linear Mold Shrinkage 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/inASTM D 955
Melt Flow  7.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
7.0 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D 1238
 21 g/10 min
@Load 10.0 kg,
Temperature 220 °C
21 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 105105ASTM D 785
Tensile Strength, Yield 35.9 MPa5210 psiASTM D 638
Tensile Modulus 2.21 GPa321 ksiASTM D 638
Flexural Strength 72.4 MPa
@Strain 5.0 %
10500 psi
@Strain 5.0 %
ASTM D 790
Flexural Modulus 2.48 GPa360 ksiASTM D 790
Izod Impact, Notched 1.71 J/cm
@Temperature 23.0 °C
3.20 ft-lb/in
@Temperature 73.4 °F
ASTM D 256
 
Thermal PropertiesMetricEnglishComments
CTE, linear 90.0 µm/m-°C50.0 µin/in-°FASTM D 696
Deflection Temperature at 0.46 MPa (66 psi) 88.9 °C192 °Funannealed; ASTM D 648
 100 °C212 °Fannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 75.6 °C168 °Funannealed; ASTM D 648
 95.0 °C203 °Fannealed; ASTM D 648
Vicat Softening Point 106 °C
@Load 1.02 kg
223 °F
@Load 2.25 lb
B/2 120C/H; ASTM D 1525
 
Processing PropertiesMetricEnglishComments
Drying Temperature 79.0 °C
@Time 7200 - 14400 sec
174 °F
@Time 2.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
INEOS Styrolution Lustran® LGA Acrylonitrile Butadiene Styrene (ABS)
SEKISUI SPI ALLEN® 6000 PMMA/ABS
INEOS Styrolution PS 6210/6211 HIPS
INEOS Styrolution PS 5600/5601 HIPS
Ineos Nova Styrosun® 3600 Weather Resistant High Impact Styrenic Polymer

PSTYR9847 / 216074

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.