MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Parker Chomerics THERM-A-GAP 570 Thermally Conductive Gap Filler
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: THERM-A-GAP™ 570 is a highly conformal, thermally conductive gap filler pad. The materials consist of an ultra-soft silicone elastomer filled with ceramic particles. THERM-A-GAP™ elastomers are used to fill air voids between PC boards or high temperature components and heat sinks, metal enclosures, and chassis. The exceptional conformability of these advanced materials enables them to blanket highly uneven surfaces, wetting out mating surfaces in order to efficiently transfer heat away from components.

Typical Applications: Telecommunications equipment; Consumer electronics; Automotive electronics (ECUs); LEDs, lighting; Power conversion; Desktop computers; laptops, servers; Handheld devices; Memory modules and Vibration dampening

Product Attributes: Best for molding complex parts and vibration dampening and Lowest outgassing

Information provided by Chomerics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.20 g/cc2.20 g/ccASTM D792
Thickness 508 - 5080 microns20.0 - 200 milASTM D374
Deformation  10 %
@Thickness 3.17 mm,
Pressure 0.0345 MPa
10 %
@Thickness 0.125 in,
Pressure 5.00 psi
0.5" diameter probe, 0.025 in/min rate; ASTM C165 MOD
 15 %
@Thickness 3.17 mm,
Pressure 0.0689 MPa
15 %
@Thickness 0.125 in,
Pressure 10.0 psi
0.5" diameter probe, 0.025 in/min rate; ASTM C165 MOD
 25 %
@Thickness 3.17 mm,
Pressure 0.172 MPa
25 %
@Thickness 0.125 in,
Pressure 25.0 psi
0.5" diameter probe, 0.025 in/min rate; ASTM C165 MOD
 25 %
@Thickness 2.54 mm,
Pressure 0.0689 MPa
25 %
@Thickness 0.100 in,
Pressure 10.0 psi
0.75" diameter round probe with 0.75" diameter circular sample; Method 2
 32 %
@Thickness 2.54 mm,
Pressure 0.138 MPa
32 %
@Thickness 0.100 in,
Pressure 20.0 psi
0.75" diameter round probe with 0.75" diameter circular sample; Method 2
 35 %
@Thickness 3.17 mm,
Pressure 0.345 MPa
35 %
@Thickness 0.125 in,
Pressure 50.0 psi
0.5" diameter probe, 0.025 in/min rate; ASTM C165 MOD
 35 %
@Thickness 2.54 mm,
Pressure 0.0689 MPa
35 %
@Thickness 0.100 in,
Pressure 10.0 psi
1" square probe with 0.5" diameter circular sample; Method 1
 40 %
@Thickness 2.54 mm,
Pressure 0.276 MPa
40 %
@Thickness 0.100 in,
Pressure 40.0 psi
0.75" diameter round probe with 0.75" diameter circular sample; Method 2
 42 %
@Thickness 2.54 mm,
Pressure 0.138 MPa
42 %
@Thickness 0.100 in,
Pressure 20.0 psi
1" square probe with 0.5" diameter circular sample; Method 1
 48 %
@Thickness 2.54 mm,
Pressure 0.276 MPa
48 %
@Thickness 0.100 in,
Pressure 40.0 psi
1" square probe with 0.5" diameter circular sample; Method 1
 48 %
@Thickness 2.54 mm,
Pressure 0.414 MPa
48 %
@Thickness 0.100 in,
Pressure 60.0 psi
0.75" diameter round probe with 0.75" diameter circular sample; Method 2
Outgassing - Total Mass Loss 0.35 %0.35 %TML; ASTM E595
Collected Volatile Condensable Material 0.090 %0.090 %ASTM E595
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore OO 2525ASTM D2240
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmASTM D257
Dielectric Constant 6.5
@Frequency 1e+6 Hz
6.5
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 7.87 kV/mm200 kV/in
Dissipation Factor 0.013
@Frequency 1e+6 Hz
0.013
@Frequency 1e+6 Hz
Chomerics Test
 
Thermal PropertiesMetricEnglishComments
CTE, linear 250 µm/m-°C139 µin/in-°FASTM E831
Specific Heat Capacity 1.00 J/g-°C0.239 BTU/lb-°FASTM E1269
Thermal Conductivity 1.50 W/m-K10.4 BTU-in/hr-ft²-°FASTM D5470
Maximum Service Temperature, Air 200 °C392 °F
Minimum Service Temperature, Air -55.0 °C-67.0 °F
Flammability, UL94 V-0V-0
 
Processing PropertiesMetricEnglishComments
Shelf Life 18.0 Month18.0 MonthFrom date of shipment A; Chomerics
 24.0 Month24.0 MonthFrom date of shipment G; Chomerics
 
Descriptive Properties
CarrierG=Fiberglass, A=Aluminum
ColorBlue

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
G-10 Fiberglass Epoxy Laminate Sheet
Parker Chomerics THERM-A-GAP 580 Thermally Conductive Gap Filler
Victrex APTIV™ 1103-050M Polyetheretherketone (PEEK) Polymer Film, Semi-Crystalline, 30% Mineral Filled
Aptek THERM-PAD 1100 Thermally conductive silicone pad
Overview of materials for Silicone Rubber

PCHOME000 / 28222

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.