MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Norplex-Micarta BR70 Phenolic Canvas Laminate Sheet
Categories: Polymer; Thermoset; Phenolic

Material Notes: BR70 is a red colored composite made from a 24 oz/sq. yd canvas which is passed through the treater twice to insure impregnation of the fibers and to obtain the resin content desired for optimal performance. The resin system is a phenolic with good impregnation qualities and cured hardness. BR70 is designed for highly loaded bearing applications, where the lubrication is provided by oil, water or a mixture.

Information provided by Norplex-Micarta

Key Words: Cotton, Phenolic, Micarta
Vendors: Norplex-Micarta is the leading manufacturer of high performance thermoset composite materials. We work directly with customers to manufacture the highest quality specialty sheet products, pre-pregs, rods and molded shapes, and tubes to meet demanding composite applications for our OEMs and fabricators around the world. Visit norplex-micarta.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.42 g/cc
@Thickness 12.7 mm
1.42 g/cc
@Thickness 0.500 in
ASTM D792
Moisture Absorption 0.0600 %
@Thickness 1.57 mm
0.0600 %
@Thickness 0.0620 in
ASTM D570 Condition A
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 95
@Thickness 6.35 mm
95
@Thickness 0.250 in
ASTM D785
Tensile Strength  77.9 MPa
@Thickness 12.7 mm
11300 psi
@Thickness 0.500 in
CrossWise; ASTM D638 Condition A
 78.6 MPa
@Thickness 12.7 mm
11400 psi
@Thickness 0.500 in
LengthWise; ASTM D638 Condition A
Flexural Strength  93.8 MPa
@Thickness 12.7 mm
13600 psi
@Thickness 0.500 in
CrossWise; ASTM D790 Condition A
 139 MPa
@Thickness 12.7 mm
20200 psi
@Thickness 0.500 in
LengthWise; ASTM D790 Condition A
Flexural Modulus  7.129 GPa
@Thickness 12.7 mm
1034 ksi
@Thickness 0.500 in
CrossWise; ASTM D790 Condition A
 9.363 GPa
@Thickness 12.7 mm
1358 ksi
@Thickness 0.500 in
LengthWise; ASTM D790 Condition A
Compressive Strength 252 MPa
@Thickness 12.7 mm
36500 psi
@Thickness 0.500 in
Flatwise; ASTM D695 Condition A
Shear Strength 95.8 MPa
@Thickness 12.7 mm
13900 psi
@Thickness 0.500 in
perpendicular; ASTM D732 Condition A
Izod Impact, Unnotched  1.51 J/cm
@Thickness 12.7 mm
2.83 ft-lb/in
@Thickness 0.500 in
CrossWise; ASTM D256 Condition E-48/50
 3.40 J/cm
@Thickness 12.7 mm
6.36 ft-lb/in
@Thickness 0.500 in
LengthWise; ASTM D256 Condition E-48/50
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 19.5 µm/m-°C
@Thickness 12.7 mm
10.8 µin/in-°F
@Thickness 0.500 in
IPC-TM 650-2.4.24
CTE, linear, Transverse to Flow 27.6 µm/m-°C
@Thickness 12.7 mm
15.3 µin/in-°F
@Thickness 0.500 in
IPC-TM 650-2.4.24
UL RTI, Mechanical with Impact 125 °C257 °FUL Bulletin 746b
Flammability, UL94 HB
@Thickness 12.7 mm
HB
@Thickness 0.500 in
 
Descriptive Properties
Bonding Strength2300[lb]; 0.5"; ASTM D229 Condition D-48/50

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Norplex-Micarta BR60 Phenolic Canvas Laminate Sheet
Mitsubishi Chemical Advanced Materials Nylatron™ MC 901 H.S. PA6
Mitsubishi Chemical Advanced Materials Nylatron™ MC™ 907 / Ertalon™ 6 PLA PA6 Unfilled Type 6 nylon
Norplex-Micarta NP310E Phenolic Cotton Laminate Sheet, NEMA CE

PNORPM076 / 192833

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.