MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Special Metals INCONEL® Alloy X-750
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: A nickel-chromium alloy similar to INCONEL alloy 600 but made precipitation hardenable by additions of aluminum and titanium. The alloy has good resistance to corrosion and oxidation along with high tensile and creep-rupture properties at temperatures to about 1300°F (700°C). Its excellent relaxation resistance is useful for high-temperature springs and bolts. Used in gas turbines, rocket engines, nuclear reactors, pressure vessels, tooling, and aircraft structures. Standard product forms are round, flats, extruded section, forging stock, plate, sheet, strip, pipe, tube, and wire.

Data provided by the manufacturer, Special Metals.

Key Words: MIL-N-7786, MIL-N-8550, MIL-S-23192, MIL-N-24114; NACE MR-01-75; AFNOR NC 15 FeT, SAE AMS 5542, 5582, 5583, 5598, 5667 - 5671, 5698, 5699, 5747, 7246, UNS N07750; BS HR505; ASTM B 637; ASME SB-637, Boiler Code Section III; Werkstoff Nr. 2.4669
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.28 g/cc0.299 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  1120 MPa
@Temperature 550 °C
162000 psi
@Temperature 1020 °F
Precipitation Hardened prior to test
 1250 MPa
@Temperature 23.0 °C
181000 psi
@Temperature 73.4 °F
Tensile Strength, Yield 850 MPa
@Strain 0.2 %
123000 psi
@Strain 0.2 %
Precipitation Hardened. Value at room temperature
 760 MPa
@Strain 0.2 %,
Temperature 550 °C
110000 psi
@Strain 0.2 %,
Temperature 1020 °F
Precipitation Hardened prior to test
Elongation at Break 30 %30 %Precipitation Hardened
 22 %
@Temperature 550 °C
22 %
@Temperature 1020 °F
Precipitation Hardened prior to test.
Rupture Strength  22.1 MPa
@Temperature 982 °C,
Time 360000 sec
3200 psi
@Temperature 1800 °F,
Time 100 hour
 110 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
16000 psi
@Temperature 1500 °F,
Time 1000 hour
 179 MPa
@Temperature 816 °C,
Time 360000 sec
26000 psi
@Temperature 1500 °F,
Time 100 hour
 469 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
68000 psi
@Temperature 1200 °F,
Time 1000 hour
 552 MPa
@Temperature 649 °C,
Time 360000 sec
80000 psi
@Temperature 1200 °F,
Time 100 hour
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000122 ohm-cm0.000122 ohm-cm
Magnetic Permeability 1.00351.0035at 200 Oersted (15.9 kA/m)
Curie Temperature -125 °C-193 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.6 µm/m-°C
@Temperature 20.0 - 100 °C
7.00 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.431 J/g-°C0.103 BTU/lb-°F
Thermal Conductivity 12.0 W/m-K83.3 BTU-in/hr-ft²-°F
Melting Point 1390 - 1430 °C2530 - 2610 °F
Solidus 1390 °C2530 °F
Liquidus 1430 °C2610 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.40 - 1.0 %0.40 - 1.0 %
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 14 - 17 %14 - 17 %
Cobalt, Co <= 1.0 %<= 1.0 %
Copper, Cu <= 0.50 %<= 0.50 %
Iron, Fe 5.0 - 9.0 %5.0 - 9.0 %
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni >= 70 %>= 70 %Including Cobalt
Niobium, Nb (Columbium, Cb) 0.70 - 1.2 %0.70 - 1.2 %Includes Ta
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.010 %<= 0.010 %
Titanium, Ti 2.25 - 2.75 %2.25 - 2.75 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 718
Special Metals INCONEL® Alloy 600
Special Metals INCONEL® Alloy 625
Special Metals NIMONIC® Alloy 90
Haynes 282® Nickel Alloy Sheet, Solution Annealed and Age-hardened

NINC35 / 17404

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.