MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Domo Technyl® A 402 H1 Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced

Material Notes: Unreinforced, very high viscosity, heat stabilized, for extrusion and injection molding. TECHNYL® A 402 H1 offers three main advantages: high impact resistance at low humidity levels, good rigidity, and excellent compression resistance. This grade is particularly suitable for the molding of plastic insulators for railway binding and for extrusion of plates and profiles.

Information provided by Rhodia; Rhodia has been acquired by Solvay.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³ISO 1183-A
Water Absorption 1.5 %
@Time 86400 sec
1.5 %
@Time 24.0 hour
ISO 62
Linear Mold Shrinkage, Flow 0.019 cm/cm0.019 in/inRhodia EP test
Linear Mold Shrinkage, Transverse 0.019 cm/cm0.019 in/inRhodia EP test
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 60.0 MPa8700 psiDAM; ISO 527 Type 1 A
Tensile Strength, Yield 60.0 MPa8700 psiConditioned; ISO 527 Type 1 A
 80.0 MPa11600 psiDAM; ISO 527 Type 1 A
Elongation at Break 60 %60 %DAM; ISO 527 Type 1 A
 250 %250 %Conditioned; ISO 527 Type 1 A
Elongation at Yield 8.0 %8.0 %DAM; ISO 527 Type 1 A
 30 %30 %Conditioned; ISO 527 Type 1 A
Tensile Modulus 1.30 GPa189 ksiConditioned; ISO 527 Type 1 A
 3.10 GPa450 ksiDAM; ISO 527 Type 1 A
Flexural Strength 75.0 MPa10900 psiConditioned; ISO 178
 140 MPa20300 psiDAM; ISO 178
Flexural Modulus 1.30 GPa189 ksiConditioned; ISO 178
 2.80 GPa406 ksiDAM; ISO 178
Izod Impact, Notched (ISO) 6.00 kJ/m²2.86 ft-lb/in²DAM; ISO 180/A
 35.0 kJ/m²16.7 ft-lb/in²Conditioned; ISO 180/A
Charpy Impact Unnotched NBNBDAM; ISO 179/1eU
 NBNBConditioned; ISO 179/1eU
Charpy Impact, Notched 0.700 J/cm²3.33 ft-lb/in²DAM; ISO 179/1eA
 3.00 J/cm²14.3 ft-lb/in²Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cmConditioned; IEC 60093
 1.00e+14 ohm-cm1.00e+14 ohm-cmDAM; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmConditioned; IEC 60093
 1.00e+12 ohm1.00e+12 ohmDAM; IEC 60093
Dielectric Strength 26.0 kV/mm660 kV/inConditioned; IEC 60243
 27.0 kV/mm686 kV/inDAM; IEC 60243
Dissipation Factor 0.0200.020DAM; IEC 60250
 0.100.10Conditioned; IEC 60250
Comparative Tracking Index 475 V475 VDAM; IEC 60112
 575 V575 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 70.0 µm/m-°C
@Temperature 23.0 - 85.0 °C
38.9 µin/in-°F
@Temperature 73.4 - 185 °F
DAM; ISO 11359
Melting Point 263 °C505 °FISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °C167 °FDAM; ISO 75-2
Oxygen Index 27 %27 %Dry; ISO 4589
Glow Wire Ignition Temperature  775 °C
@Thickness 1.60 mm
1430 °F
@Thickness 0.0630 in
DAM; IEC 60695-2-13
 775 °C
@Thickness 3.20 mm
1430 °F
@Thickness 0.126 in
DAM; IEC 60695-2-13
Glow Wire Flammability Index  960 °C
@Thickness 0.800 mm
1760 °F
@Thickness 0.0315 in
DAM; IEC 60695-2-12
 960 °C
@Thickness 1.60 mm
1760 °F
@Thickness 0.0630 in
DAM; IEC 60695-2-12
 960 °C
@Thickness 3.20 mm
1760 °F
@Thickness 0.126 in
DAM; IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 260 - 270 °C500 - 518 °F
Middle Barrel Temperature 270 - 280 °C518 - 536 °F
Front Barrel Temperature 280 - 290 °C536 - 554 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
Drying Temperature 80.0 °C176 °F
Moisture Content <= 0.20 %<= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Zytel® 42A NC010 PA66
Domo Technyl® A 205F Nylon 66, EH0
Domo Technyl® B 50H1 Nylon 66/6, Flame Retardant, EH0
Domo Technyl® A 246M Nylon 66, Impact Grade, EH0
Domo Technyl® A218 Heat Stabilized Nylon 66

PRHO09m / 123360

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.