MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow Surlyn® 9320 Zinc Ionomer
Categories: Polymer; Thermoplastic; Ionomer

Material Notes: Surlyn® 9320 is a zinc ionomer thermoplastic resin. It is available for use in conventional extrusion and injection equipment, to create various sheets or shapes. Surlyn® 9320 thermoplastic resin is an advanced ethylene/acid/acrylate terpolymer, in which some of the MAA acid groups have been partially neutralized with zinc ions.

This former DuPont product line is now a Dow product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.960 g/cc0.0347 lb/in³ASTM D792, ISO 1183
Melt Flow 0.80 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.80 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238, ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4040ASTM D2240, ISO 868
Abrasive Hardness 169169NBS Index, ASTM D1630
Tensile Strength at Break 15.9 MPa
@Temperature 23.0 °C
2310 psi
@Temperature 73.4 °F
ASTM D638, ISO 527-2
Tensile Strength, Yield 3.50 MPa
@Temperature 23.0 °C
508 psi
@Temperature 73.4 °F
ASTM D638
Elongation at Break 525 %
@Temperature 23.0 °C
525 %
@Temperature 73.4 °F
ASTM D638, ISO 527-2
Flexural Modulus 0.0296 GPa
@Temperature 23.0 °C
4.29 ksi
@Temperature 73.4 °F
ASTM D790
 
Thermal PropertiesMetricEnglishComments
Melting Point 37.0 °C98.6 °FFreezing Point; ASTM D3418, ISO 3146
 70.0 °C158 °FASTM D3418, ISO 3146
Vicat Softening Point 48.0 °C118 °FASTM D1525, ISO 306
 
Optical PropertiesMetricEnglishComments
Haze 12.3 %
@Thickness 6.35 mm
12.3 %
@Thickness 0.250 in
ASTM D1003
 
Processing PropertiesMetricEnglishComments
Processing Temperature <= 285 °C<= 545 °F
Melt Temperature 185 - 285 °C365 - 545 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow Surlyn® 7930 Ionomer Resin, Lithium
Dow Surlyn® 6320 Magnesium Ionomer
Dow Surlyn® 1707 Sodium Ionomer
Dow Surlyn® 8528 Sodium Ionomer
Dow Surlyn® E185SB Ionomer Resin

PDTA4978 / 170418

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.