MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 4043-H14
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 4000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A94043; ISO AlSi5; Aluminium 4043-H14; AA4043-H14; Al4043-H14
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.69 g/cc0.0972 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 4646500 kg load with 10 mm ball. Calculated value.
Tensile Strength, Ultimate 170 MPa24700 psi
Tensile Strength, Yield 165 MPa23900 psi
Elongation at Break 1.3 %
@Diameter 3.20 mm
1.3 %
@Diameter 0.126 in
in 5 cm, wire
Poissons Ratio 0.340.34Estimated from trends in similar Al alloys.
Shear Strength 106 MPa15400 psiCalculated value.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000440 ohm-cm0.00000440 ohm-cmEstimated from other heat treatments.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  22.1 µm/m-°C
@Temperature 20.0 - 100 °C
12.3 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 23.7 µm/m-°C
@Temperature 20.0 - 300 °C
13.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.850 J/g-°C0.203 BTU/lb-°FEstimated from trends in similar Al alloys.
Thermal Conductivity 150 W/m-K1040 BTU-in/hr-ft²-°FEstimated from other heat treatments.
Melting Point 573.9 - 632 °C1065 - 1170 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 573.9 °C1065 °FAA; Typical
Liquidus 632 °C1170 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 349 °C660 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 92.3 - 95.5 %92.3 - 95.5 %As remainder
Beryllium, Be <= 0.0008 %<= 0.0008 %welding electrode and filler wire only
Copper, Cu <= 0.30 %<= 0.30 %
Iron, Fe <= 0.80 %<= 0.80 %
Magnesium, Mg <= 0.05 %<= 0.05 %
Manganese, Mn <= 0.05 %<= 0.05 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 4.5 - 6.0 %4.5 - 6.0 %
Titanium, Ti <= 0.20 %<= 0.20 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 4043-O
Aluminum 5052-O
Aluminum 4043-H16
Aluminum 4043-H18
Aluminum 4045

MA4043H14 / 9085

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.