MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Low Density Polyethylene (LDPE), Film Grade
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Film Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Low Density Polyethylene (LDPE), Film Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.902 - 1.00 g/cc0.0326 - 0.0361 lb/in³Average value: 0.923 g/cc Grade Count:543
Water Absorption 0.0100 %0.0100 %Average value: 0.0100 % Grade Count:17
Moisture Absorption at Equilibrium 0.0100 %0.0100 %Average value: 0.0100 % Grade Count:17
Water Vapor Transmission 0.990 - 16.0 g/m²/day0.0638 - 1.03 g/100 in²/dayAverage value: 12.8 g/m²/day Grade Count:21
Oxygen Transmission Rate 2000 - 6820 cc/m²/day129 - 439 cc/100 in²/dayAverage value: 4670 cc/m²/day Grade Count:21
Nitrogen Transmission 3500 - 7500 cc-mm/m²-24hr-atm8890 - 19100 cc-mil/100 in²-24hr-atmAverage value: 4500 cc-mm/m²-24hr-atm Grade Count:4
Environmental Stress Crack Resistance 1.50 - 500 hour1.50 - 500 hourAverage value: 155 hour Grade Count:12
Vinyl Acetate Content 2.50 - 6.60 %2.50 - 6.60 %Average value: 4.67 % Grade Count:26
Thickness 12.7 - 300 microns0.500 - 11.8 milAverage value: 52.4 microns Grade Count:261
Melt Flow 0.120 - 65.0 g/10 min0.120 - 65.0 g/10 minAverage value: 2.40 g/10 min Grade Count:525
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 80.0 - 99.080.0 - 99.0Average value: 87.6 Grade Count:7
Hardness, Shore D 41.0 - 60.041.0 - 60.0Average value: 49.3 Grade Count:72
Tensile Strength, Ultimate 7.00 - 34.5 MPa1020 - 5000 psiAverage value: 13.0 MPa Grade Count:102
Film Tensile Strength at Yield, MD 6.21 - 28.0 MPa900 - 4060 psiAverage value: 11.5 MPa Grade Count:235
Film Tensile Strength at Yield, TD 5.86 - 100 MPa850 - 14500 psiAverage value: 11.6 MPa Grade Count:245
Tensile Strength, Yield 8.00 - 22.0 MPa1160 - 3190 psiAverage value: 11.6 MPa Grade Count:105
Film Elongation at Break, MD 100 - 650 %100 - 650 %Average value: 322 % Grade Count:469
Film Elongation at Break, TD 249 - 1330 %249 - 1330 %Average value: 590 % Grade Count:468
Film Elongation at Yield, MD 5.60 - 425 %5.60 - 425 %Average value: 53.1 % Grade Count:16
Film Elongation at Yield, TD 5.00 - 600 %5.00 - 600 %Average value: 75.0 % Grade Count:16
Elongation at Break 50.0 - 1000 %50.0 - 1000 %Average value: 448 % Grade Count:110
Elongation at Yield 4.00 - 100 %4.00 - 100 %Average value: 34.7 % Grade Count:30
Modulus of Elasticity 0.140 - 0.480 GPa20.3 - 69.6 ksiAverage value: 0.245 GPa Grade Count:115
Flexural Yield Strength 160 - 290 MPa23200 - 42100 psiAverage value: 220 MPa Grade Count:15
Flexural Modulus 0.124 - 0.690 GPa18.0 - 100 ksiAverage value: 0.251 GPa Grade Count:24
Secant Modulus 0.00114 - 1.35 GPa0.166 - 196 ksiAverage value: 0.305 GPa Grade Count:17
Secant Modulus, MD 0.0179 - 0.372 GPa2.60 - 54.0 ksiAverage value: 0.196 GPa Grade Count:284
Secant Modulus, TD 0.0221 - 0.414 GPa3.20 - 60.0 ksiAverage value: 0.222 GPa Grade Count:284
Izod Impact, Notched (ISO) 5.00 - 5.00 kJ/m²
@Temperature -30.0 - -30.0 °C
2.38 - 2.38 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 5.00 kJ/m² Grade Count:1
Tensile Impact Strength 23.0 - 147 kJ/m²10.9 - 69.9 ft-lb/in²Average value: 51.2 kJ/m² Grade Count:5
 86.0 - 86.0 kJ/m²
@Temperature -30.0 - -30.0 °C
40.9 - 40.9 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 86.0 kJ/m² Grade Count:1
Tensile Impact 130 - 350 J/cm244 - 656 ft-lb/inAverage value: 228 J/cm Grade Count:17
Dart Drop, Total Energy 16.0 - 19.0 J11.8 - 14.0 ft-lbAverage value: 17.1 J Grade Count:5
 6.20 - 26.0 J
@Temperature -40.0 - -40.0 °C
4.57 - 19.2 ft-lb
@Temperature -40.0 - -40.0 °F
Average value: 16.9 J Grade Count:5
Puncture Energy 0.203 - 7.00 J0.150 - 5.16 ft-lbAverage value: 1.72 J Grade Count:49
Coefficient of Friction 0.0900 - 1.500.0900 - 1.50Average value: 0.473 Grade Count:213
Tear Strength, Total 2.00 - 4.00 N0.450 - 0.899 lb (f)Average value: 3.00 N Grade Count:7
Tear Strength 20.0 - 373 kN/m114 - 2130 pliAverage value: 59.8 kN/m Grade Count:31
Elmendorf Tear Strength MD 8.83 - 1070 g8.83 - 1070 gAverage value: 296 g Grade Count:211
Elmendorf Tear Strength TD 8.34 - 1370 g8.34 - 1370 gAverage value: 232 g Grade Count:226
Elmendorf Tear Strength, MD 1.20 - 18.1 g/micron30.5 - 460 g/milAverage value: 7.45 g/micron Grade Count:167
Elmendorf Tear Strength, TD 2.10 - 100 g/micron53.3 - 2540 g/milAverage value: 7.36 g/micron Grade Count:180
Dart Drop Total Energy 13.0 - 31.0 J/cm0.0244 - 0.0581 ft-lb/milAverage value: 23.3 J/cm Grade Count:8
Dart Drop 1.30 - 100 g/micron33.0 - 2540 g/milAverage value: 4.96 g/micron Grade Count:166
Dart Drop Test 18.0 - 1500 g0.0397 - 3.31 lbAverage value: 168 g Grade Count:391
Film Tensile Strength at Break, MD 14.0 - 200 MPa2030 - 29000 psiAverage value: 27.1 MPa Grade Count:452
Film Tensile Strength at Break, TD 11.0 - 57.0 MPa1600 - 8270 psiAverage value: 21.4 MPa Grade Count:448
Heat Seal Strength 3.00 - 10.8 g/25 mm0.00661 - 0.0238 lb/inAverage value: 6.64 g/25 mm Grade Count:13
Heat Seal Strength Initiation Temperature 100 - 105 °C212 - 221 °FAverage value: 104 °C Grade Count:8
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 500 - 1.00e+15 ohm-cm500 - 1.00e+15 ohm-cmAverage value: 5.67e+14 ohm-cm Grade Count:31
Surface Resistance 31000 - 1.00e+14 ohm31000 - 1.00e+14 ohmAverage value: 5.67e+13 ohm Grade Count:31
Static Decay 2.00 sec2.00 secAverage value: 2.00 sec Grade Count:13
Dielectric Constant 2.302.30Average value: 2.30 Grade Count:17
Dissipation Factor 0.0002000.000200Average value: 0.000200 Grade Count:17
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:17
 
Thermal PropertiesMetricEnglishComments
CTE, linear 180 - 230 µm/m-°C100 - 128 µin/in-°FAverage value: 206 µm/m-°C Grade Count:17
Melting Point 97.8 - 218 °C208 - 424 °FAverage value: 113 °C Grade Count:274
Crystallization Temperature 95.0 - 104 °C203 - 219 °FAverage value: 98.4 °C Grade Count:11
Deflection Temperature at 0.46 MPa (66 psi) 38.3 - 45.0 °C101 - 113 °FAverage value: 42.4 °C Grade Count:19
Vicat Softening Point 70.0 - 109 °C158 - 228 °FAverage value: 94.6 °C Grade Count:299
Brittleness Temperature -76.0 - -32.0 °C-105 - -25.6 °FAverage value: -73.6 °C Grade Count:70
Flammability, UL94 HBHBGrade Count:17
Oxygen Index 17.0 %17.0 %Average value: 17.0 % Grade Count:17
 
Optical PropertiesMetricEnglishComments
Haze 0.650 - 55.0 %0.650 - 55.0 %Average value: 8.55 % Grade Count:457
Gloss 8.20 - 135 %8.20 - 135 %Average value: 69.2 % Grade Count:432
Transmission, Visible 55.0 - 90.0 %55.0 - 90.0 %Average value: 88.8 % Grade Count:30
 
Processing PropertiesMetricEnglishComments
Processing Temperature 140 - 400 °C284 - 752 °FAverage value: 190 °C Grade Count:105
Die Temperature 150 - 290 °C302 - 554 °FAverage value: 203 °C Grade Count:3
Melt Temperature 110 - 260 °C230 - 500 °FAverage value: 189 °C Grade Count:107
Die Opening 0.0635 - 0.152 cm0.0250 - 0.0600 inAverage value: 0.103 cm Grade Count:16

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for High Density Polyethylene (HDPE), Film Grade
Overview of materials for Linear Low Density Polyethylene (LLDPE), Film Grade
Overview of materials for Low Density Polyethylene (LDPE), Molded
Overview of materials for Low Density Polyethylene (LDPE), Extrusion Grade
Overview of materials for Medium Density Polyethylene (MDPE), Film Grade

O3805 / 78249

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.