MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AFE Technologies Cronite 37Ni/18Cr No. HR5
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy; Iron Base

Material Notes: High temperature nickel alloy castings. Applications include heat treatment and handling products, furnace products, tubes, power generation, and petrochemical industries.

Information provided by AFE Technologies/North American Cronite, Inc.

Key Words: Cronite 37/18; Werkstoff 1.4865
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 460 MPa66700 psiAs Cast
Tensile Strength, Yield 240 MPa34800 psiAs Cast
Elongation at Break 6.0 %6.0 %As Cast; 5.65 A0.5
Rupture Strength  3.20 MPa
@Temperature 1150 °C,
Time 3.60e+7 sec
464 psi
@Temperature 2100 °F,
Time 10000 hour
Stress Rupture
 4.70 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
682 psi
@Temperature 2010 °F,
Time 10000 hour
Stress Rupture
 7.00 MPa
@Temperature 1050 °C,
Time 3.60e+7 sec
1020 psi
@Temperature 1920 °F,
Time 10000 hour
Stress Rupture
 10.5 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
1520 psi
@Temperature 1830 °F,
Time 10000 hour
Stress Rupture
 16.0 MPa
@Temperature 950 °C,
Time 3.60e+7 sec
2320 psi
@Temperature 1740 °F,
Time 10000 hour
Stress Rupture
 23.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
3340 psi
@Temperature 1650 °F,
Time 10000 hour
Stress Rupture
 32.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
4640 psi
@Temperature 1560 °F,
Time 10000 hour
Stress Rupture
 42.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
6090 psi
@Temperature 1470 °F,
Time 10000 hour
Stress Rupture
 56.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
8120 psi
@Temperature 1380 °F,
Time 10000 hour
Stress Rupture
 75.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
10900 psi
@Temperature 1290 °F,
Time 10000 hour
Stress Rupture
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.40 %0.40 %
Chromium, Cr 18 %18 %
Iron, Fe 41.8 %41.8 %As Remainder
Manganese, Mn 1.0 %1.0 %
Nickel, Ni 37 %37 %
Silicon, Si 1.8 %1.8 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Alloy 713LC Cast Nickel Superalloy
Aluminum 6061-T6; 6061-T651
AFE Technologies Cronite 37Ni/18Cr/Nb No. HR32
AFE Technologies Cronite 34Ni/25Cr/Nb No. HR 33 Nb
Cast Stainless Steel HU, UNS N08004

NCRON02 / 15987

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.