MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Polycasa Acryl® KR 2006/1 Acrylic, Impact Grade
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, Impact Modified, Molded

Material Notes: Impact-modified grade for highly stressed parts; highest impact and notched-impact resistance; can be mixed with general-purpose grades to get the desired toughness; highly resistant to stress cracking.

Data was collected by ISO methods.

Quinn Manufacturing Group rebranded its Plastics Division as Polycasa in 2013.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³
Moisture Absorption at Equilibrium 0.40 %0.40 %
Linear Mold Shrinkage, Flow 0.0065 cm/cm0.0065 in/in
Melt Flow 0.90 g/10 min
@Load 3.80 kg,
Temperature 230 °C
0.90 g/10 min
@Load 8.38 lb,
Temperature 446 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 45.0 MPa6530 psi
Elongation at Break 45 %45 %
Elongation at Yield 5.0 %5.0 %
Tensile Modulus 1.80 GPa261 ksi
Charpy Impact Unnotched 8.00 J/cm²38.1 ft-lb/in²
Charpy Impact, Notched 0.700 J/cm²3.33 ft-lb/in²
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cm
Surface Resistance 1.00e+14 ohm1.00e+14 ohm
Dielectric Constant  2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
 3.2
@Frequency 100 Hz
3.2
@Frequency 100 Hz
Dielectric Strength 60.0 kV/mm1520 kV/in
Dissipation Factor  0.030
@Frequency 1e+6 Hz
0.030
@Frequency 1e+6 Hz
 0.040
@Frequency 100 Hz
0.040
@Frequency 100 Hz
Comparative Tracking Index 600 V600 V
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C
@Temperature 20.0 °C
61.1 µin/in-°F
@Temperature 68.0 °F
Deflection Temperature at 0.46 MPa (66 psi) 90.0 °C194 °F
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C185 °F
Vicat Softening Point 98.0 °C208 °F
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
Oxygen Index 18 %18 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Polycasa Acryl® KR 2007/1 Acrylic
Polycasa Acryl® KR 2014/1 Acrylic, Impact Grade
Polycasa Acryl® G 77 E Acrylic, Extrusion Grade
Polycasa Acryl® G 77 Acrylic, Injection Molding Grade
Polycasa Acryl® KR 2015/1 Acrylic, Impact Grade

PSF018 / 66576

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.