MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type S14800 Stainless Steel condition CH900, 72.5% cold reduction
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless; T S10000 Series Stainless Steel

Material Notes: A precipitation-hardening stainless steel. Maintains high strength at elevated temperatures.

Key Words: UNS S14800, AMS 5601, AMS 5603; Precipitation Hardening
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.70 g/cc0.278 lb/in³In condition SRH950, 7.83 in condition A
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 567567Converted from Rockwell C hardness.
Hardness, Knoop 631631Converted from Rockwell C hardness.
Hardness, Rockwell C 55.555.5
Hardness, Vickers 604604Converted from Rockwell C hardness.
Tensile Strength, Ultimate 2137 MPa309900 psi
Tensile Strength, Yield 2103 MPa
@Strain 0.2 %
305000 psi
@Strain 0.2 %
Elongation at Break 0.00 %0.00 %in 50 mm
Modulus of Elasticity 200 GPa29000 ksiTypical for stainless steel
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.50 µm/m-°C
@Temperature 21.0 - 93.0 °C
5.28 µin/in-°F
@Temperature 69.8 - 199 °F
 10.6 µm/m-°C
@Temperature 21.0 - 205 °C
5.89 µin/in-°F
@Temperature 69.8 - 401 °F
 11.2 µm/m-°C
@Temperature 21.0 - 315 °C
6.22 µin/in-°F
@Temperature 69.8 - 599 °F
 11.5 µm/m-°C
@Temperature 21.0 - 540 °C
6.39 µin/in-°F
@Temperature 69.8 - 1000 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.75 - 1.5 %0.75 - 1.5 %
Carbon, C <= 0.050 %<= 0.050 %
Chromium, Cr 13.75 - 15 %13.75 - 15 %
Iron, Fe 73 %73 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 2.0 - 3.0 %2.0 - 3.0 %
Nickel, Ni 7.75 - 8.75 %7.75 - 8.75 %
Phosphorus, P <= 0.015 %<= 0.015 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.010 %<= 0.010 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900
AK Steel 17-7 PH® Precipitation Hardening Stainless Steel, Condition RH 950
AK Steel 17-7 PH® Precipitation Hardening Stainless Steel, Condition A
AK Steel 17-7 PH® Precipitation Hardening Stainless Steel, Condition CH 900
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 925

MQM14BD / 13509

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.