MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celanex® 1400FC PBT, Unfilled
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Celanex 1400FC is a general purpose, unreinforced polybutylene terephthalate with a good balance of mechanical properties and processability for use in food contact applications. Celanex 1400FC is a high flow material.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.31 g/cc1.31 g/ccASTM D792
Density 1.31 g/cc0.0473 lb/in³ISO 1183
Water Absorption 0.080 %
@Temperature 22.8 °C
0.080 %
@Temperature 73.0 °F
24hr immersion; ASTM D570
Linear Mold Shrinkage, Flow 0.018 - 0.020 cm/cm0.018 - 0.020 in/inASTM D955
 0.018 - 0.020 cm/cm0.018 - 0.020 in/inISO 294-4
Melt Flow 50 g/10 min50 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7272ISO 2039-2
Tensile Strength at Break 55.2 MPa8000 psiASTM D638
Tensile Strength, Yield 55.2 MPa8000 psiASTM D638
 60.0 MPa8700 psi50mm/min; ISO 527-2/1A
Elongation at Break 38 %38 %
 50 %50 %ASTM D638
Elongation at Yield 4.0 %4.0 %50mm/min; ISO 527-2/1A
Tensile Modulus 2.70 GPa392 ksi50mm/min; ISO 527-2/1A
Flexural Strength 80.0 MPa11600 psiISO 178
 82.7 MPa12000 psiASTM D790
Flexural Modulus 2.20 GPa319 ksiISO 178
 2.28 GPa330 ksiASTM D790
Izod Impact, Notched 0.320 J/cm0.600 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 3.70 kJ/m²1.76 ft-lb/in²ISO 180/1A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
 1.00e+15 ohm-cm1.00e+15 ohm-cmASTM D257
Surface Resistance 1.00e+15 ohm1.00e+15 ohmIEC 60093
Dielectric Constant 3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 15.0 kV/mm381 kV/inIEC 60243-1
 15.7 kV/mm400 kV/inshort term; ASTM D149
Dissipation Factor  0.0010
@Frequency 1000 Hz
0.0010
@Frequency 1000 Hz
ASTM D150
 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 190 sec190 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FISO 11359-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1,-2,-3
 225 °C437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 142 °C288 °FISO 75-1, -2
 154 °C310 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 54.4 °C130 °FASTM D648
 58.0 °C136 °FISO 75-1, -2
Glass Transition Temp, Tg 60.0 °C140 °FISO 11357-1,-2,-3
Flammability, UL94 HBHB
 HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 65.0 - 93.0 °C149 - 199 °Fcavity
 250 - 260 °C482 - 500 °Fhot runner
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 260 °C464 - 500 °F
Die Temperature 250 - 260 °C482 - 500 °F
Melt Temperature 243 °C469 °FISO 294
 235 - 260 °C455 - 500 °F
Mold Temperature 82.0 °C180 °FISO 294
Injection Velocity 300 mm/sec11.8 in/secISO 294
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4.00 hour4.00 hour
Moisture Content <= 0.020 %<= 0.020 %
Hold Pressure 48.0 MPa6960 psiISO 294
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Celanex® 1400A PBT, Unfilled
Celanese Celanex® 1602Z PBT, Unfilled
Celanese Celanex® 1500A PBT, Unfilled
Celanese Celanex® 1462Z PBT, 30% Glass Reinforced
Celanese Celanex® 1600A PBT, Unfilled

PHCQ002 / 178457

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.