MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

NatureWorks® Ingeo™ 3052D Lubricated, High Flow Biopolymer
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polylactic Acid (PLA) Biopolymer

Material Notes: NatureWorks® PLA polymer 2003D is a thermoplastic resin derived from annually renewable resources. It is designed for injection molding applications where the requirements are clarity with heat deflection temperatures below 120ºF (49ºC). Sample uses include food service products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.24 g/cc1.24 g/ccASTM D792
Viscosity Measurement 3.3
@Temperature 30.0 °C
3.3
@Temperature 86.0 °F
1.0 g/dl in chloroform; Relative Viscosity
Linear Mold Shrinkage 0.003 - 0.005 cm/cm0.003 - 0.005 in/in
Melt Flow 14 g/10 min
@Load 2.16 kg,
Temperature 210 °C
14 g/10 min
@Load 4.76 lb,
Temperature 410 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 54.0 MPa7830 psiASTM D882
Tensile Strength, Yield 62.0 MPa8990 psiASTM D882
Elongation at Break 3.5 %3.5 %ASTM D882
Tensile Modulus 3.72 GPa540 ksiASTM D882
Flexural Strength 108 MPa15700 psiASTM D790
Flexural Modulus 3.55 GPa515 ksiASTM D790
Izod Impact, Notched 0.1600 J/cm0.2997 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 145 - 160 °C293 - 320 °FPeak; ASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 55.0 °C131 °FASTM E2092
Glass Transition Temp, Tg 55.0 - 60.0 °C131 - 140 °FASTM D3418
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 90 %90 %Thickness Unknown
 
Processing PropertiesMetricEnglishComments
Feed Temperature 165 °C329 °F
Nozzle Temperature 205 °C401 °F
Melt Temperature 200 °C392 °F
Mold Temperature 25.0 °C77.0 °F
Moisture Content <= 0.025 %<= 0.025 %
Back Pressure 0.345 - 0.689 MPa50.0 - 100 psi
Screw Speed 100 - 175 rpm100 - 175 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
NatureWorks® Ingeo™ 3001D Injection Grade PLA
NatureWorks® Ingeo™ 3251D Injection Grade PLA
NatureWorks® Ingeo™ AW 300D Injection Grade Biopolymer
NatureWorks® Ingeo™ 2002D Extrusion Grade PLA
Overview of materials for Polylactic Acid (PLA) Biopolymer

PNATU72 / 135567

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.