MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum 2219-T87 (Extended Creep-Rupture Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
This designation is considered the sole original alloy for this alloy family.
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T87; AA2219-T87
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.84 g/cc0.103 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 130130500 kg load with 10 mm ball
Hardness, Knoop 163163Converted from Brinell Hardness Value
Hardness, Rockwell A 49.549.5Converted from Brinell Hardness Value
Hardness, Rockwell B 8080Converted from Brinell Hardness Value
Hardness, Vickers 149149Converted from Brinell Hardness Value
Tensile Strength, Ultimate 476 MPa69000 psiAA; Typical
 >= 420 MPa
@Thickness 101.6 - 127 mm
>= 60900 psi
@Thickness 4.001 - 5.00 in
Sheet and plate
 >= 425 MPa
@Thickness 76.23 - 102 mm
>= 61600 psi
@Thickness 3.001 - 4.00 in
Sheet and plate
 >= 440 MPa
@Thickness 0.508 - 6.32 mm
>= 63800 psi
@Thickness 0.0200 - 0.249 in
Sheet and plate
 >= 440 MPa
@Thickness 6.35 - 76.2 mm
>= 63800 psi
@Thickness 0.250 - 3.00 in
Sheet and plate
Tensile Strength, Yield 393 MPa57000 psiAA; Typical
 >= 340 MPa
@Thickness 101.6 - 127 mm
>= 49300 psi
@Thickness 4.001 - 5.00 in
Sheet and plate
 >= 345 MPa
@Thickness 76.23 - 102 mm
>= 50000 psi
@Thickness 3.001 - 4.00 in
Sheet and plate
 >= 350 MPa
@Thickness 6.35 - 76.2 mm
>= 50800 psi
@Thickness 0.250 - 3.00 in
Sheet and plate
 >= 360 MPa
@Thickness 0.508 - 6.32 mm
>= 52200 psi
@Thickness 0.0200 - 0.249 in
Sheet and plate
Elongation at Break  3.0 %
@Thickness 101.6 - 127 mm
3.0 %
@Thickness 4.001 - 5.00 in
Sheet and plate
 4.0 %
@Thickness 76.23 - 102 mm
4.0 %
@Thickness 3.001 - 4.00 in
Sheet and plate
 5.0 - 6.0 %
@Thickness 0.508 - 6.32 mm
5.0 - 6.0 %
@Thickness 0.0200 - 0.249 in
Sheet and plate
 6.0 - 7.0 %
@Thickness 6.35 - 76.2 mm
6.0 - 7.0 %
@Thickness 0.250 - 3.00 in
Sheet and plate
 10 %
@Thickness 1.59 mm
10 %
@Thickness 0.0625 in
AA; Typical
Creep Strength  6.00 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
870 psi
@Temperature 698 °F,
Time 1000 hour
0.1% creep
 8.00 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1160 psi
@Temperature 698 °F,
Time 1000 hour
0.2% creep
 8.00 MPa
@Temperature 370 °C,
Time 360000 sec
1160 psi
@Temperature 698 °F,
Time 100 hour
0.1% creep
 11.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1600 psi
@Temperature 698 °F,
Time 1000 hour
0.5% creep
 11.0 MPa
@Temperature 370 °C,
Time 360000 sec
1600 psi
@Temperature 698 °F,
Time 100 hour
0.2% creep
 12.0 MPa
@Temperature 370 °C,
Time 36000 sec
1740 psi
@Temperature 698 °F,
Time 10.0 hour
0.1% creep
 13.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1890 psi
@Temperature 698 °F,
Time 1000 hour
1% creep
 17.0 MPa
@Temperature 370 °C,
Time 360000 sec
2470 psi
@Temperature 698 °F,
Time 100 hour
0.5% creep
 17.0 MPa
@Temperature 370 °C,
Time 36000 sec
2470 psi
@Temperature 698 °F,
Time 10.0 hour
0.2% creep
 18.0 MPa
@Temperature 370 °C,
Time 3600 sec
2610 psi
@Temperature 698 °F,
Time 1.00 hour
0.1% creep
 20.0 MPa
@Temperature 370 °C,
Time 360000 sec
2900 psi
@Temperature 698 °F,
Time 100 hour
1% creep
 23.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
3340 psi
@Temperature 599 °F,
Time 1000 hour
0.1% creep
 26.0 MPa
@Temperature 370 °C,
Time 36000 sec
3770 psi
@Temperature 698 °F,
Time 10.0 hour
0.5% creep
 26.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
3770 psi
@Temperature 599 °F,
Time 1000 hour
0.2% creep
 28.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
4060 psi
@Temperature 599 °F,
Time 1000 hour
0.5% creep
 30.0 MPa
@Temperature 370 °C,
Time 36000 sec
4350 psi
@Temperature 698 °F,
Time 10.0 hour
1% creep
 31.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
4500 psi
@Temperature 599 °F,
Time 1000 hour
1% creep
 32.0 MPa
@Temperature 370 °C,
Time 3600 sec
4640 psi
@Temperature 698 °F,
Time 1.00 hour
0.2% creep
 34.0 MPa
@Temperature 315 °C,
Time 360000 sec
4930 psi
@Temperature 599 °F,
Time 100 hour
0.1% creep
 34.0 MPa
@Temperature 370 °C,
Time 360 sec
4930 psi
@Temperature 698 °F,
Time 0.100 hour
0.1% creep
 41.0 MPa
@Temperature 370 °C,
Time 3600 sec
5950 psi
@Temperature 698 °F,
Time 1.00 hour
0.5% creep
 45.0 MPa
@Temperature 370 °C,
Time 3600 sec
6530 psi
@Temperature 698 °F,
Time 1.00 hour
1% creep
 45.0 MPa
@Temperature 315 °C,
Time 360000 sec
6530 psi
@Temperature 599 °F,
Time 100 hour
0.2% creep
 48.0 MPa
@Temperature 370 °C,
Time 360 sec
6960 psi
@Temperature 698 °F,
Time 0.100 hour
0.2% creep
 52.0 MPa
@Temperature 315 °C,
Time 360000 sec
7540 psi
@Temperature 599 °F,
Time 100 hour
0.5% creep
 52.0 MPa
@Temperature 370 °C,
Time 360 sec
7540 psi
@Temperature 698 °F,
Time 0.100 hour
0.5% creep
 52.0 MPa
@Temperature 315 °C,
Time 36000 sec
7540 psi
@Temperature 599 °F,
Time 10.0 hour
0.1% creep
 55.0 MPa
@Temperature 315 °C,
Time 360000 sec
7980 psi
@Temperature 599 °F,
Time 100 hour
1% creep
 55.0 MPa
@Temperature 370 °C,
Time 360 sec
7980 psi
@Temperature 698 °F,
Time 0.100 hour
1% creep
 59.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
8560 psi
@Temperature 500 °F,
Time 1000 hour
0.1% creep
 62.0 MPa
@Temperature 315 °C,
Time 36000 sec
8990 psi
@Temperature 599 °F,
Time 10.0 hour
0.2% creep
 66.0 MPa
@Temperature 315 °C,
Time 3600 sec
9570 psi
@Temperature 599 °F,
Time 1.00 hour
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
10000 psi
@Temperature 500 °F,
Time 1000 hour
0.2% creep
 69.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
10000 psi
@Temperature 446 °F,
Time 1000 hour
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 360000 sec
10000 psi
@Temperature 500 °F,
Time 100 hour
0.1% creep
 76.0 MPa
@Temperature 315 °C,
Time 36000 sec
11000 psi
@Temperature 599 °F,
Time 10.0 hour
0.5% creep
 83.0 MPa
@Temperature 315 °C,
Time 360 sec
12000 psi
@Temperature 599 °F,
Time 0.100 hour
0.1% creep
 83.0 MPa
@Temperature 315 °C,
Time 36000 sec
12000 psi
@Temperature 599 °F,
Time 10.0 hour
1% creep
 83.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
12000 psi
@Temperature 446 °F,
Time 1000 hour
0.2% creep
 83.0 MPa
@Temperature 315 °C,
Time 3600 sec
12000 psi
@Temperature 599 °F,
Time 1.00 hour
0.2% creep
 83.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
12000 psi
@Temperature 401 °F,
Time 1000 hour
0.1% creep
 83.0 MPa
@Temperature 230 °C,
Time 360000 sec
12000 psi
@Temperature 446 °F,
Time 100 hour
0.1% creep
 83.0 MPa
@Temperature 260 °C,
Time 36000 sec
12000 psi
@Temperature 500 °F,
Time 10.0 hour
0.1% creep
 90.0 MPa
@Temperature 260 °C,
Time 360000 sec
13100 psi
@Temperature 500 °F,
Time 100 hour
0.2% creep
 97.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
14100 psi
@Temperature 500 °F,
Time 1000 hour
0.5% creep
 97.0 MPa
@Temperature 315 °C,
Time 3600 sec
14100 psi
@Temperature 599 °F,
Time 1.00 hour
0.5% creep
 97.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
14100 psi
@Temperature 401 °F,
Time 1000 hour
0.2% creep
 97.0 MPa
@Temperature 315 °C,
Time 360 sec
14100 psi
@Temperature 599 °F,
Time 0.100 hour
0.2% creep
 97.0 MPa
@Temperature 205 °C,
Time 360000 sec
14100 psi
@Temperature 401 °F,
Time 100 hour
0.1% creep
 97.0 MPa
@Temperature 230 °C,
Time 36000 sec
14100 psi
@Temperature 446 °F,
Time 10.0 hour
0.1% creep
 105 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
15200 psi
@Temperature 500 °F,
Time 1000 hour
1% creep
 105 MPa
@Temperature 315 °C,
Time 3600 sec
15200 psi
@Temperature 599 °F,
Time 1.00 hour
1% creep
 105 MPa
@Temperature 315 °C,
Time 360 sec
15200 psi
@Temperature 599 °F,
Time 0.100 hour
0.5% creep
 105 MPa
@Temperature 230 °C,
Time 360000 sec
15200 psi
@Temperature 446 °F,
Time 100 hour
0.2% creep
 105 MPa
@Temperature 260 °C,
Time 36000 sec
15200 psi
@Temperature 500 °F,
Time 10.0 hour
0.2% creep
 105 MPa
@Temperature 260 °C,
Time 3600 sec
15200 psi
@Temperature 500 °F,
Time 1.00 hour
0.1% creep
 110 MPa
@Temperature 315 °C,
Time 360 sec
16000 psi
@Temperature 599 °F,
Time 0.100 hour
1% creep
 110 MPa
@Temperature 260 °C,
Time 360000 sec
16000 psi
@Temperature 500 °F,
Time 100 hour
0.5% creep
 110 MPa
@Temperature 205 °C,
Time 36000 sec
16000 psi
@Temperature 401 °F,
Time 10.0 hour
0.1% creep
 115 MPa
@Temperature 260 °C,
Time 360000 sec
16700 psi
@Temperature 500 °F,
Time 100 hour
1% creep
 115 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
16700 psi
@Temperature 446 °F,
Time 1000 hour
0.5% creep
 115 MPa
@Temperature 205 °C,
Time 360000 sec
16700 psi
@Temperature 401 °F,
Time 100 hour
0.2% creep
 115 MPa
@Temperature 230 °C,
Time 36000 sec
16700 psi
@Temperature 446 °F,
Time 10.0 hour
0.2% creep
 115 MPa
@Temperature 230 °C,
Time 3600 sec
16700 psi
@Temperature 446 °F,
Time 1.00 hour
0.1% creep
 125 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
18100 psi
@Temperature 446 °F,
Time 1000 hour
1% creep
 125 MPa
@Temperature 230 °C,
Time 360000 sec
18100 psi
@Temperature 446 °F,
Time 100 hour
0.5% creep
 125 MPa
@Temperature 260 °C,
Time 36000 sec
18100 psi
@Temperature 500 °F,
Time 10.0 hour
0.5% creep
 125 MPa
@Temperature 260 °C,
Time 3600 sec
18100 psi
@Temperature 500 °F,
Time 1.00 hour
0.2% creep
 125 MPa
@Temperature 260 °C,
Time 360 sec
18100 psi
@Temperature 500 °F,
Time 0.100 hour
0.1% creep
 130 MPa
@Temperature 260 °C,
Time 36000 sec
18900 psi
@Temperature 500 °F,
Time 10.0 hour
1% creep
 130 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
18900 psi
@Temperature 401 °F,
Time 1000 hour
0.5% creep
 140 MPa
@Temperature 230 °C,
Time 360000 sec
20300 psi
@Temperature 446 °F,
Time 100 hour
1% creep
 140 MPa
@Temperature 230 °C,
Time 360 sec
20300 psi
@Temperature 446 °F,
Time 0.100 hour
0.1% creep
 140 MPa
@Temperature 260 °C,
Time 3600 sec
20300 psi
@Temperature 500 °F,
Time 1.00 hour
0.5% creep
 140 MPa
@Temperature 205 °C,
Time 36000 sec
20300 psi
@Temperature 401 °F,
Time 10.0 hour
0.2% creep
 140 MPa
@Temperature 230 °C,
Time 3600 sec
20300 psi
@Temperature 446 °F,
Time 1.00 hour
0.2% creep
 140 MPa
@Temperature 260 °C,
Time 360 sec
20300 psi
@Temperature 500 °F,
Time 0.100 hour
0.2% creep
 140 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
20300 psi
@Temperature 302 °F,
Time 1000 hour
0.1% creep
 140 MPa
@Temperature 205 °C,
Time 3600 sec
20300 psi
@Temperature 401 °F,
Time 1.00 hour
0.1% creep
 145 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
21000 psi
@Temperature 401 °F,
Time 1000 hour
1% creep
 145 MPa
@Temperature 260 °C,
Time 3600 sec
21000 psi
@Temperature 500 °F,
Time 1.00 hour
1% creep
 145 MPa
@Temperature 205 °C,
Time 360000 sec
21000 psi
@Temperature 401 °F,
Time 100 hour
0.5% creep
 145 MPa
@Temperature 230 °C,
Time 36000 sec
21000 psi
@Temperature 446 °F,
Time 10.0 hour
0.5% creep
 150 MPa
@Temperature 260 °C,
Time 360 sec
21800 psi
@Temperature 500 °F,
Time 0.100 hour
0.5% creep
 160 MPa
@Temperature 230 °C,
Time 36000 sec
23200 psi
@Temperature 446 °F,
Time 10.0 hour
1% creep
 160 MPa
@Temperature 260 °C,
Time 360 sec
23200 psi
@Temperature 500 °F,
Time 0.100 hour
1% creep
 165 MPa
@Temperature 205 °C,
Time 360000 sec
23900 psi
@Temperature 401 °F,
Time 100 hour
1% creep
 165 MPa
@Temperature 230 °C,
Time 3600 sec
23900 psi
@Temperature 446 °F,
Time 1.00 hour
0.5% creep
 165 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
23900 psi
@Temperature 302 °F,
Time 1000 hour
0.2% creep
 165 MPa
@Temperature 205 °C,
Time 3600 sec
23900 psi
@Temperature 401 °F,
Time 1.00 hour
0.2% creep
 165 MPa
@Temperature 230 °C,
Time 360 sec
23900 psi
@Temperature 446 °F,
Time 0.100 hour
0.2% creep
 165 MPa
@Temperature 150 °C,
Time 360000 sec
23900 psi
@Temperature 302 °F,
Time 100 hour
0.1% creep
 165 MPa
@Temperature 205 °C,
Time 360 sec
23900 psi
@Temperature 401 °F,
Time 0.100 hour
0.1% creep
 170 MPa
@Temperature 230 °C,
Time 3600 sec
24700 psi
@Temperature 446 °F,
Time 1.00 hour
1% creep
 170 MPa
@Temperature 205 °C,
Time 36000 sec
24700 psi
@Temperature 401 °F,
Time 10.0 hour
0.5% creep
 180 MPa
@Temperature 230 °C,
Time 360 sec
26100 psi
@Temperature 446 °F,
Time 0.100 hour
0.5% creep
 185 MPa
@Temperature 205 °C,
Time 36000 sec
26800 psi
@Temperature 401 °F,
Time 10.0 hour
1% creep
 195 MPa
@Temperature 230 °C,
Time 360 sec
28300 psi
@Temperature 446 °F,
Time 0.100 hour
1% creep
 200 MPa
@Temperature 205 °C,
Time 3600 sec
29000 psi
@Temperature 401 °F,
Time 1.00 hour
0.5% creep
 200 MPa
@Temperature 150 °C,
Time 360000 sec
29000 psi
@Temperature 302 °F,
Time 100 hour
0.2% creep
 200 MPa
@Temperature 205 °C,
Time 360 sec
29000 psi
@Temperature 401 °F,
Time 0.100 hour
0.2% creep
 205 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
29700 psi
@Temperature 302 °F,
Time 1000 hour
0.5% creep
 205 MPa
@Temperature 150 °C,
Time 36000 sec
29700 psi
@Temperature 302 °F,
Time 10.0 hour
0.1% creep
 215 MPa
@Temperature 205 °C,
Time 3600 sec
31200 psi
@Temperature 401 °F,
Time 1.00 hour
1% creep
 230 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
33400 psi
@Temperature 302 °F,
Time 1000 hour
1% creep
 230 MPa
@Temperature 205 °C,
Time 360 sec
33400 psi
@Temperature 401 °F,
Time 0.100 hour
0.5% creep
 235 MPa
@Temperature 150 °C,
Time 360000 sec
34100 psi
@Temperature 302 °F,
Time 100 hour
0.5% creep
 235 MPa
@Temperature 150 °C,
Time 36000 sec
34100 psi
@Temperature 302 °F,
Time 10.0 hour
0.2% creep
 240 MPa
@Temperature 205 °C,
Time 360 sec
34800 psi
@Temperature 401 °F,
Time 0.100 hour
1% creep
 240 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
34800 psi
@Temperature 212 °F,
Time 1000 hour
0.1% creep
 240 MPa
@Temperature 150 °C,
Time 3600 sec
34800 psi
@Temperature 302 °F,
Time 1.00 hour
0.1% creep
 250 MPa
@Temperature 150 °C,
Time 360000 sec
36300 psi
@Temperature 302 °F,
Time 100 hour
1% creep
 260 MPa
@Temperature 150 °C,
Time 36000 sec
37700 psi
@Temperature 302 °F,
Time 10.0 hour
0.5% creep
 260 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
37700 psi
@Temperature 212 °F,
Time 1000 hour
0.2% creep
 260 MPa
@Temperature 150 °C,
Time 3600 sec
37700 psi
@Temperature 302 °F,
Time 1.00 hour
0.2% creep
 260 MPa
@Temperature 100 °C,
Time 360000 sec
37700 psi
@Temperature 212 °F,
Time 100 hour
0.1% creep
 270 MPa
@Temperature 150 °C,
Time 360 sec
39200 psi
@Temperature 302 °F,
Time 0.100 hour
0.1% creep
 275 MPa
@Temperature 150 °C,
Time 36000 sec
39900 psi
@Temperature 302 °F,
Time 10.0 hour
1% creep
 290 MPa
@Temperature 150 °C,
Time 3600 sec
42100 psi
@Temperature 302 °F,
Time 1.00 hour
0.5% creep
 290 MPa
@Temperature 100 °C,
Time 360000 sec
42100 psi
@Temperature 212 °F,
Time 100 hour
0.2% creep
 290 MPa
@Temperature 150 °C,
Time 360 sec
42100 psi
@Temperature 302 °F,
Time 0.100 hour
0.2% creep
 290 MPa
@Temperature 100 °C,
Time 36000 sec
42100 psi
@Temperature 212 °F,
Time 10.0 hour
0.1% creep
 295 MPa
@Temperature 150 °C,
Time 3600 sec
42800 psi
@Temperature 302 °F,
Time 1.00 hour
1% creep
 295 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
42800 psi
@Temperature 212 °F,
Time 1000 hour
0.5% creep
 305 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
44200 psi
@Temperature 212 °F,
Time 1000 hour
1% creep
 305 MPa
@Temperature 100 °C,
Time 36000 sec
44200 psi
@Temperature 212 °F,
Time 10.0 hour
0.2% creep
 310 MPa
@Temperature 100 °C,
Time 360000 sec
45000 psi
@Temperature 212 °F,
Time 100 hour
0.5% creep
 310 MPa
@Temperature 150 °C,
Time 360 sec
45000 psi
@Temperature 302 °F,
Time 0.100 hour
0.5% creep
 310 MPa
@Temperature 100 °C,
Time 3600 sec
45000 psi
@Temperature 212 °F,
Time 1.00 hour
0.1% creep
 315 MPa
@Temperature 100 °C,
Time 360000 sec
45700 psi
@Temperature 212 °F,
Time 100 hour
1% creep
 315 MPa
@Temperature 150 °C,
Time 360 sec
45700 psi
@Temperature 302 °F,
Time 0.100 hour
1% creep
 325 MPa
@Temperature 100 °C,
Time 36000 sec
47100 psi
@Temperature 212 °F,
Time 10.0 hour
0.5% creep
 325 MPa
@Temperature 100 °C,
Time 3600 sec
47100 psi
@Temperature 212 °F,
Time 1.00 hour
0.2% creep
 325 MPa
@Temperature 100 °C,
Time 360 sec
47100 psi
@Temperature 212 °F,
Time 0.100 hour
0.1% creep
 330 MPa
@Temperature 100 °C,
Time 36000 sec
47900 psi
@Temperature 212 °F,
Time 10.0 hour
1% creep
 340 MPa
@Temperature 100 °C,
Time 3600 sec
49300 psi
@Temperature 212 °F,
Time 1.00 hour
0.5% creep
 340 MPa
@Temperature 100 °C,
Time 360 sec
49300 psi
@Temperature 212 °F,
Time 0.100 hour
0.2% creep
 345 MPa
@Temperature 100 °C,
Time 3600 sec
50000 psi
@Temperature 212 °F,
Time 1.00 hour
1% creep
 345 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
50000 psi
@Temperature 75.2 °F,
Time 1000 hour
0.1% creep
 350 MPa
@Temperature 100 °C,
Time 360 sec
50800 psi
@Temperature 212 °F,
Time 0.100 hour
0.5% creep
 350 MPa
@Temperature 24.0 °C,
Time 360000 sec
50800 psi
@Temperature 75.2 °F,
Time 100 hour
0.1% creep
 360 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
52200 psi
@Temperature 75.2 °F,
Time 1000 hour
0.2% creep
 360 MPa
@Temperature 24.0 °C,
Time 36000 sec
52200 psi
@Temperature 75.2 °F,
Time 10.0 hour
0.1% creep
 365 MPa
@Temperature 100 °C,
Time 360 sec
52900 psi
@Temperature 212 °F,
Time 0.100 hour
1% creep
 365 MPa
@Temperature 24.0 °C,
Time 360000 sec
52900 psi
@Temperature 75.2 °F,
Time 100 hour
0.2% creep
 365 MPa
@Temperature 24.0 °C,
Time 3600 sec
52900 psi
@Temperature 75.2 °F,
Time 1.00 hour
0.1% creep
 370 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
53700 psi
@Temperature 75.2 °F,
Time 1000 hour
0.5% creep
 370 MPa
@Temperature 24.0 °C,
Time 36000 sec
53700 psi
@Temperature 75.2 °F,
Time 10.0 hour
0.2% creep
 370 MPa
@Temperature 24.0 °C,
Time 360 sec
53700 psi
@Temperature 75.2 °F,
Time 0.100 hour
0.1% creep
 380 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
55100 psi
@Temperature 75.2 °F,
Time 1000 hour
1% creep
 380 MPa
@Temperature 24.0 °C,
Time 360000 sec
55100 psi
@Temperature 75.2 °F,
Time 100 hour
0.5% creep
 380 MPa
@Temperature 24.0 °C,
Time 3600 sec
55100 psi
@Temperature 75.2 °F,
Time 1.00 hour
0.2% creep
 385 MPa
@Temperature 24.0 °C,
Time 36000 sec
55800 psi
@Temperature 75.2 °F,
Time 10.0 hour
0.5% creep
 385 MPa
@Temperature 24.0 °C,
Time 360 sec
55800 psi
@Temperature 75.2 °F,
Time 0.100 hour
0.2% creep
 395 MPa
@Temperature 24.0 °C,
Time 360000 sec
57300 psi
@Temperature 75.2 °F,
Time 100 hour
1% creep
 400 MPa
@Temperature 24.0 °C,
Time 3600 sec
58000 psi
@Temperature 75.2 °F,
Time 1.00 hour
0.5% creep
 405 MPa
@Temperature 24.0 °C,
Time 36000 sec
58700 psi
@Temperature 75.2 °F,
Time 10.0 hour
1% creep
 420 MPa
@Temperature 24.0 °C,
Time 360 sec
60900 psi
@Temperature 75.2 °F,
Time 0.100 hour
0.5% creep
 425 MPa
@Temperature 24.0 °C,
Time 3600 sec
61600 psi
@Temperature 75.2 °F,
Time 1.00 hour
1% creep
 450 MPa
@Temperature 24.0 °C,
Time 360 sec
65300 psi
@Temperature 75.2 °F,
Time 0.100 hour
1% creep
Rupture Strength  17.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
2470 psi
@Temperature 698 °F,
Time 1000 hour
 23.0 MPa
@Temperature 370 °C,
Time 360000 sec
3340 psi
@Temperature 698 °F,
Time 100 hour
 34.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
4930 psi
@Temperature 599 °F,
Time 1000 hour
 34.0 MPa
@Temperature 370 °C,
Time 36000 sec
4930 psi
@Temperature 698 °F,
Time 10.0 hour
 48.0 MPa
@Temperature 370 °C,
Time 3600 sec
6960 psi
@Temperature 698 °F,
Time 1.00 hour
 59.0 MPa
@Temperature 370 °C,
Time 360 sec
8560 psi
@Temperature 698 °F,
Time 0.100 hour
 62.0 MPa
@Temperature 315 °C,
Time 360000 sec
8990 psi
@Temperature 599 °F,
Time 100 hour
 90.0 MPa
@Temperature 315 °C,
Time 36000 sec
13100 psi
@Temperature 599 °F,
Time 10.0 hour
 105 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
15200 psi
@Temperature 500 °F,
Time 1000 hour
 105 MPa
@Temperature 315 °C,
Time 3600 sec
15200 psi
@Temperature 599 °F,
Time 1.00 hour
 115 MPa
@Temperature 315 °C,
Time 360 sec
16700 psi
@Temperature 599 °F,
Time 0.100 hour
 125 MPa
@Temperature 260 °C,
Time 360000 sec
18100 psi
@Temperature 500 °F,
Time 100 hour
 145 MPa
@Temperature 260 °C,
Time 36000 sec
21000 psi
@Temperature 500 °F,
Time 10.0 hour
 150 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
21800 psi
@Temperature 401 °F,
Time 1000 hour
 150 MPa
@Temperature 230 °C,
Time 360000 sec
21800 psi
@Temperature 446 °F,
Time 100 hour
 160 MPa
@Temperature 260 °C,
Time 3600 sec
23200 psi
@Temperature 500 °F,
Time 1.00 hour
 170 MPa
@Temperature 230 °C,
Time 36000 sec
24700 psi
@Temperature 446 °F,
Time 10.0 hour
 170 MPa
@Temperature 260 °C,
Time 360 sec
24700 psi
@Temperature 500 °F,
Time 0.100 hour
 180 MPa
@Temperature 205 °C,
Time 360000 sec
26100 psi
@Temperature 401 °F,
Time 100 hour
 185 MPa
@Temperature 230 °C,
Time 3600 sec
26800 psi
@Temperature 446 °F,
Time 1.00 hour
 205 MPa
@Temperature 205 °C,
Time 36000 sec
29700 psi
@Temperature 401 °F,
Time 10.0 hour
 206 MPa
@Temperature 230 °C,
Time 360 sec
29900 psi
@Temperature 446 °F,
Time 0.100 hour
 230 MPa
@Temperature 205 °C,
Time 3600 sec
33400 psi
@Temperature 401 °F,
Time 1.00 hour
 235 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
34100 psi
@Temperature 302 °F,
Time 1000 hour
 255 MPa
@Temperature 205 °C,
Time 360 sec
37000 psi
@Temperature 401 °F,
Time 0.100 hour
 260 MPa
@Temperature 150 °C,
Time 360000 sec
37700 psi
@Temperature 302 °F,
Time 100 hour
 290 MPa
@Temperature 150 °C,
Time 36000 sec
42100 psi
@Temperature 302 °F,
Time 10.0 hour
 315 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
45700 psi
@Temperature 212 °F,
Time 1000 hour
 315 MPa
@Temperature 150 °C,
Time 3600 sec
45700 psi
@Temperature 302 °F,
Time 1.00 hour
 330 MPa
@Temperature 100 °C,
Time 360000 sec
47900 psi
@Temperature 212 °F,
Time 100 hour
 345 MPa
@Temperature 150 °C,
Time 360 sec
50000 psi
@Temperature 302 °F,
Time 0.100 hour
 350 MPa
@Temperature 100 °C,
Time 36000 sec
50800 psi
@Temperature 212 °F,
Time 10.0 hour
 380 MPa
@Temperature 100 °C,
Time 3600 sec
55100 psi
@Temperature 212 °F,
Time 1.00 hour
 400 MPa
@Temperature 100 °C,
Time 360 sec
58000 psi
@Temperature 212 °F,
Time 0.100 hour
 420 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
60900 psi
@Temperature 75.2 °F,
Time 1000 hour
 435 MPa
@Temperature 24.0 °C,
Time 360000 sec
63100 psi
@Temperature 75.2 °F,
Time 100 hour
 450 MPa
@Temperature 24.0 °C,
Time 36000 sec
65300 psi
@Temperature 75.2 °F,
Time 10.0 hour
 455 MPa
@Temperature 24.0 °C,
Time 3600 sec
66000 psi
@Temperature 75.2 °F,
Time 1.00 hour
 460 MPa
@Temperature 24.0 °C,
Time 360 sec
66700 psi
@Temperature 75.2 °F,
Time 0.100 hour
 1130 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
164000 psi
@Temperature 446 °F,
Time 1000 hour
Modulus of Elasticity 73.1 GPa10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Notched Tensile Strength 379 MPa55000 psi2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Fatigue Strength 103 MPa
@# of Cycles 5.00e+8
15000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPa3920 ksiEstimated from similar Al alloys.
Shear Strength 280 MPa40600 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000582 ohm-cm
@Temperature 20.0 °C
0.00000582 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.6 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.3 µm/m-°C
@Temperature 20.0 - 100 °C
12.4 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
12.5 µin/in-°F
@Temperature 68.0 - 212 °F
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.0 µin/in-°F
@Temperature 68.0 - 392 °F
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
13.4 µin/in-°F
@Temperature 68.0 - 572 °F
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
13.6 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.864 J/g-°C0.207 BTU/lb-°F
Thermal Conductivity 121 W/m-K840 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 543 - 643 °C1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 543 °C1010 °FAA; Typical
Liquidus 643 °C1190 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 535 °C995 °F
Aging Temperature 163 - 191 °C325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 91.5 - 93.8 %91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %5.8 - 6.8 %
Iron, Fe <= 0.30 %<= 0.30 %
Magnesium, Mg <= 0.02 %<= 0.02 %
Manganese, Mn 0.20 - 0.40 %0.20 - 0.40 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.20 %<= 0.20 %
Titanium, Ti 0.02 - 0.10 %0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %0.05 - 0.15 %
Zinc, Zn <= 0.10 %<= 0.10 %
Zirconium, Zr 0.10 - 0.25 %0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2618-T61 (Includes Creep/Rupture Data)
Aluminum 7178-T6; 7178-T651 (Included Creep/Rupture Data)
AISI 8620H Steel, quenched from 900°C (1650°F), tempered at 650°C (1200°F), Low temp impact properties
Aluminum 6069-T6, Cold Impact Extruded Cylinder, Minimum Tensile Values
Aluminum 2218-T61 (Includes Creep/Rupture/Fatigue Data)

MA2219T87a / 170644

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.