MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lubrizol ESTANE® GP55DT Ether Based Thermoplastic Polyurethane  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Ether Grade

Material Notes: Type: Estane® GP 55DT is an aromatic polyether-based thermoplastic polyurethane (TPU).

Appearance: Translucent spherical pellets

Uses: Injection molding parts, animal identification tags

Available in Europe

Information provided by Lubrizol.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.16 g/cc1.16 g/ccISO 2781
Maximum Moisture Content 0.0500.050
Melt Flow 15 - 35 g/10 min
@Load 8.70 kg,
Temperature 210 °C
15 - 35 g/10 min
@Load 19.2 lb,
Temperature 410 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9898ISO 868
Hardness, Shore D 5555ISO 868
Tensile Strength, Ultimate 46.0 MPa6670 psiISO 37
Elongation at Break 500 %500 %ISO 37
Tensile Modulus 0.0910 GPa13.2 ksiISO 527
50% Modulus 14.5 MPa
@Strain 50 %
14.5 MPa
@Strain 50 %
ISO 37
100% Modulus 17.0 MPa
@Strain 100 %
2470 psi
@Strain 100 %
ISO 37
300% Modulus 28.0 MPa
@Strain 300 %
4060 psi
@Strain 300 %
ISO 37
Rebound 32 %32 %ISO 4662
Tear Strength 133 kN/m759 pliwith incision; ISO 34B
 163 kN/m930 pliwithout incision; ISO 34B
Abrasion 3030mm3; ISO 4649
Compression Set  26 %
@Temperature 22.0 °C,
Time 252000 sec
26 %
@Temperature 71.6 °F,
Time 70.0 hour
ISO 815
 44 %
@Temperature 70.0 °C,
Time 86400 sec
44 %
@Temperature 158 °F,
Time 24.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 132 °C270 °FA50; ISO 306
 
Processing PropertiesMetricEnglishComments
Feed Temperature 40.0 °C104 °FInjection
Nozzle Temperature 210 - 220 °C410 - 428 °FInjection
Zone 1 200 - 210 °C392 - 410 °FInjection
Zone 2 210 - 220 °C410 - 428 °FInjection
Zone 3 210 - 220 °C410 - 428 °FInjection
Zone 4 215 - 225 °C419 - 437 °FInjection
Drying Temperature 100 °C212 °F
Dry Time 2.00 - 3.00 hour2.00 - 3.00 hour
Dew Point -30.0 °C-22.0 °F

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol ESTANE® GP95AE Ester Based Thermoplastic Polyurethane
Lubrizol Estane® 2355-55DE Thermoplastic Polyurethane
Lubrizol Estane® R198A-8 Thermoplastic Polyurethane
Lubrizol Estane® S395A Thermoplastic Polyurethane
Lubrizol Estane® S398A Thermoplastic Polyurethane

PNOVEON148 / 55417

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.