MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil HD 4504 Blow Molding Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Blow Molding Grade

Material Notes: Product Description: ExxonMobil™ HD 4504 is a blow molding high density polyethylene copolymer offering exceptional stress cracking resistance and impact performance.

Availability: Africa & Middle East, Latin America, North America and South America

Additive:

  • Thermal Stabilizer: Yes
  • Antistatic: No
Applications:
  • Agricultural Products
  • Food packaging
  • Household and Industrial chemical containers
  • Pharmaceutical Packaging
Information provided by ExxonMobil Chemical

Key Words: Paxon™ AA45-004
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.945 g/cc0.0341 lb/in³ASTM D4883
ESCR 100% Igepal® >= 1000 hour>= 1000 hourASTM D1693
Melt Flow 0.35 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.35 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 24.1 MPa3500 psiASTM D638
Elongation at Break 900 %900 %ASTM D638
Flexural Modulus 1.03 GPa150 ksiMethod1, Procedure A (1"x3"x0.125"), Tangent calculation; ASTM D790
Tensile Impact Strength 231 kJ/m²110 ft-lb/in²ASTM D1822
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 121 °C250 °FASTM D1525
Brittleness Temperature <= -76.1 °C<= -105 °FASTM D746
 
Processing PropertiesMetricEnglishComments
Melt Temperature 191 °C375 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Alathon® L5040 High Density Polyethylene, Blow Molding/Extrusion Grade
ExxonMobil HD 5003 Blow Molding Resin
ExxonMobil PP3155E3 Polypropylene Copolymer
ExxonMobil PP4031E2 Polypropylene Impact Copolymer
LyondellBasell Pro-fax SG702 Polypropylene Impact Copolymer

PEXB089 / 37394

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.