MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow DOWLEX™ 2045G Linear Low Density Polyethylene
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes: DOWLEX™ 2045G resin is designed for the production of a wide variety of industrial and consumer films (though it is not recommended for silage stretch film). The product also delivers very good processability on conventional LLDPE machinery.

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³ASTM D792
Thickness 50.8 microns2.00 mil
Melt Flow 1.0 g/10 min1.0 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 10.89 MPa1579 psiASTM D882
Film Tensile Strength at Yield, TD 12.29 MPa1783 psiASTM D882
Film Elongation at Break, MD 827 %827 %ASTM D882
Film Elongation at Break, TD 889 %889 %ASTM D882
Secant Modulus, MD 0.1944 GPa28.20 ksi2% Secant; ASTM D882
Secant Modulus, TD 0.2326 GPa33.74 ksi2% Secant; ASTM D882
Impact 235235[ft-lbf/in3]; Puncture Resistance; Dow Method
 41764176[ft-lbf/in3]; Toughness MD; ASTM D882
 42414241[ft-lbf/in3]; Toughness TD; ASTM D882
Elmendorf Tear Strength MD 902 g902 gASTM D1922
Elmendorf Tear Strength TD 1200 g1200 gASTM D1922
Elmendorf Tear Strength, MD 17.8 g/micron451 g/milASTM D1922
Elmendorf Tear Strength, TD 23.6 g/micron600 g/milASTM D1922
Dart Drop Test 288 g0.635 lbMethod A; ASTM D1709
Film Tensile Strength at Break, MD 55.11 MPa7993 psiASTM D882
Film Tensile Strength at Break, TD 49.81 MPa7224 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 122 °C252 °FDow Method (DSC)
Vicat Softening Point 108 °C226 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 10 %10 %ASTM D1003
Gloss 60 %60 %45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow DOWLEX™ 2045.11G Linear Low Density Polyethylene
Borealis Borstar® FB2230 LLDPE for Film
Dow ELITE™ 5100G Enhanced Polyethylene Resin
Dow DOWLEX™ 2047G Linear Low Density Polyethylene
Dow DOWLEX™ 2049 Linear Low Density Polyethylene, Food Grade

PDOW1306 / 30524

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.