MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Zirconium Carbide, ZrC
Categories: Ceramic; Carbide

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 6.56 g/cc0.237 lb/in³theoretical
 6.73 g/cc0.243 lb/in³
Molecular Weight 103.235 g/mol103.235 g/mol
 
Mechanical PropertiesMetricEnglishComments
Knoop Microhardness 18301830100 g load
Vickers Microhardness 2310 - 25202310 - 252050 g load
 26002600100 g load
Tensile Strength, Ultimate  14.0 - 48.0 MPa
@Temperature 1925 °C
2030 - 6960 psi
@Temperature 3497 °F
 83.0 - 96.0 MPa
@Temperature 980 °C
12000 - 13900 psi
@Temperature 1800 °F
 69.0 - 110 MPa
@Temperature 1590 °C
10000 - 16000 psi
@Temperature 2890 °F
 89.0 - 110 MPa
@Temperature 1200 °C
12900 - 16000 psi
@Temperature 2190 °F
Modulus of Elasticity 385 - 406 GPa55800 - 58900 ksisingle crystal
 345 - 400 GPa
@Temperature 20.0 - 1230 °C
50000 - 58000 ksi
@Temperature 68.0 - 2250 °F
single crystal
Compressive Strength  255 MPa
@Temperature 1200 °C
37000 psi
@Temperature 2190 °F
 488 MPa
@Temperature 1000 °C
70800 psi
@Temperature 1830 °F
 826 - 2958 MPa
@Temperature 22.0 °C
120000 - 429000 psi
@Temperature 71.6 °F
Poissons Ratio 0.190.19
 0.200.20single crystal
Shear Modulus 165 - 200 GPa23900 - 29000 ksisingle crystal
 
Electrical PropertiesMetricEnglishComments
Magnetic Susceptibility -0.0000260-0.0000260cm^3/mol
 
Thermal PropertiesMetricEnglishComments
Melting Point 3400 °C6150 °FAlternate references for m.p.
 3532 °C6390 °FAlternate references for m.p.
 
Descriptive Properties
CAS Number12020-14-3
ColorGray
Crystal StructureCubic

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tungsten Carbide, WC
Tantalum Carbide, TaC
Titanium Carbide, TiC
Niobium Carbide, NbC
Tungsten Carbide, W2C

BCZrCA / 167

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.