MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger TECASINT 1011 Polyimide (PI)
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: TECASINT is a range of non-melting high temperature polyimides characterized by high strength over a wide range of temperatures, good long term thermal stability, minimal thermal expansion and excellent wear resistance among other things. The TECASINT 2000 series offers these enhanced thermal properties along with lower moisture absorption, a higher degree of toughness, and better machining properties. TECASINT 2011 is unfilled, while TECASINT 2021 contains 15% graphite which offer improved wear resistance and a lower coefficient of friction. TECASINT 2000 series with their superior physical properties, are ideal for application in the aerospace, nuclear, automotive, electrical/electronics, and chemical processing industries.
    Main Features
  • High thermal and mechanical capacity
  • Good radiation-resistance
  • Broad chemical compatibility
  • Easily machined to tight tolerances
  • Very good electrical insulation
  • Very creep resistant
  • Low outgassing
  • Wear-resistant
  • Sensitive to hydrolysis in higher thermal range
  • Flame retardant according to UL94 V-0

    Applications
  • Cryogenics
  • Electrical engineering
  • Precision engineering
  • Mechanical engineering
  • Nuclear and vacuum technology
  • Semiconductor technology
  • Electronics
  • Aircraft and aerospace industries
  • Food technology

Preferred Fields

Insulators, switch parts, valve faces, friction rings, chain guides, gripper finger for hot glass, sole plate, wear parts

Information Provided by Ensinger, Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.34 g/cc
@Temperature 23.0 °C
0.0484 lb/in³
@Temperature 73.4 °F
DIN 53 479
Water Absorption  1.08 %
@Temperature 23.0 °C,
Time 86400 sec
1.08 %
@Temperature 73.4 °F,
Time 24.0 hour
EN ISO 62
 3.29 %
@Temperature 80.0 °C,
Time 86400 sec
3.29 %
@Temperature 176 °F,
Time 24.0 hour
EN ISO 62
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 90
@Temperature 23.0 °C
90
@Temperature 73.4 °F
DIN 53 505
Tensile Strength, Yield 116 MPa
@Temperature 23.0 °C
16800 psi
@Temperature 73.4 °F
EN ISO 527
Elongation at Break 9.0 %
@Temperature 23.0 °C
9.0 %
@Temperature 73.4 °F
EN ISO 527
Tensile Modulus 4.00 GPa
@Temperature 23.0 °C
580 ksi
@Temperature 73.4 °F
EN ISO 527
Flexural Strength 210 MPa
@Temperature 23.0 °C
30500 psi
@Temperature 73.4 °F
EN ISO 178
Flexural Modulus 3.448 GPa
@Temperature 23.0 °C
500.1 ksi
@Temperature 73.4 °F
EN ISO 178
Flexural Strain at Yield 7.3 %7.3 %EN ISO 178
Compressive Yield Strength 240 MPa34800 psi10% Strain; EN ISO 604
Compressive Strength 556 MPa
@Temperature 23.0 °C
80600 psi
@Temperature 73.4 °F
EN ISO 604
Compressive Modulus 4.00 GPa
@Temperature 23.0 °C
580 ksi
@Temperature 73.4 °F
EN ISO 604
Charpy Impact Unnotched 7.58 J/cm²36.1 ft-lb/in²EN ISO 179
Charpy Impact, Notched 0.330 J/cm²
@Temperature 23.0 °C
1.57 ft-lb/in²
@Temperature 73.4 °F
EN ISO 179
Compression Set 45 %45 %Compression at Break; EN ISO 604
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm
@Temperature 23.0 °C
1.00e+17 ohm-cm
@Temperature 73.4 °F
IEC 60093
Surface Resistance 1.00e+16 ohm
@Temperature 23.0 °C
1.00e+16 ohm
@Temperature 73.4 °F
IEC 60093
Dielectric Constant  3.1
@Frequency 2.70e+7 Hz,
Temperature 23.0 °C
3.1
@Frequency 2.70e+7 Hz,
Temperature 73.4 °F
IEC 60250
 3.5
@Frequency 50 Hz,
Temperature 23.0 °C
3.5
@Frequency 50 Hz,
Temperature 73.4 °F
IEC 60250
Dielectric Strength 20.0 kV/mm
@Temperature 23.0 °C
508 kV/in
@Temperature 73.4 °F
DC; ISO 60243-1
Dissipation Factor  0.0010
@Frequency 50 Hz,
Temperature 23.0 °C
0.0010
@Frequency 50 Hz,
Temperature 73.4 °F
DIN 53 483
 0.0030
@Frequency 2.70e+7 Hz,
Temperature 23.0 °C
0.0030
@Frequency 2.70e+7 Hz,
Temperature 73.4 °F
DIN 53 483
 
Thermal PropertiesMetricEnglishComments
CTE, linear  43.0 µm/m-°C
@Temperature 50.0 - 200 °C
23.9 µin/in-°F
@Temperature 122 - 392 °F
DIN 53 752
 53.0 µm/m-°C
@Temperature 200 - 300 °C
29.4 µin/in-°F
@Temperature 392 - 572 °F
DIN 53 752
CTE, linear, Transverse to Flow  43.0 µm/m-°C
@Temperature 50.0 - 200 °C
23.9 µin/in-°F
@Temperature 122 - 392 °F
DIN 53 752
 53.0 µm/m-°C
@Temperature 200 - 300 °C
29.4 µin/in-°F
@Temperature 392 - 572 °F
DIN 53 752
Specific Heat Capacity 1.04 J/g-°C0.249 BTU/lb-°F
Thermal Conductivity 0.220 W/m-K
@Temperature 40.0 °C
1.53 BTU-in/hr-ft²-°F
@Temperature 104 °F
ISO 8302
Maximum Service Temperature, Air 300 °C572 °F
Deflection Temperature at 1.8 MPa (264 psi) 368 °C694 °FDIN 53 461
Glass Transition Temp, Tg 368 °C694 °FDMTA
Flammability, UL94 V-0V-0
 
Descriptive Properties
ColorBlack
DIN-AbbreviationPI

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ensinger TECASINT 8001 Polytetrafluoroethylene (PTFE) + Polyimide, 20% (PI)
Ensinger TECASINT 1101 Polyimide (PI)
Ensinger TECASINT™ 2021 Polyimide, Brown (PI)
Mitsubishi Chemical Advanced Materials Ertalyte™ PET Polyester-semi-crystalline thermoplastic, extruded
Ensinger TECASINT 1021 Polyimide, 15% Graphite Filled (PI)

PENSIN044 / 98105

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.