MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Makrolon® 6717 Polycarbonate, Flame Retardant Grade
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Extruded

Material Notes: MVR (300 °C/1.2 kg) 3.0 cm³/10 min; flame retardant; UL 94V-0/2.0 mm; high viscosity; branched; UV stabilized; easy release; injection molding - melt temperature 280 - 320 °C; extrusion; available in transparent, translucent and opaque colors

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.660 g/cc0.0238 lb/in³pellets; ISO 60
Density 1.20 g/cc0.0434 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.12 %0.12 %ISO 62
Water Absorption at Saturation 0.30 %0.30 %ISO 62
Water Vapor Transmission 15.0 g/m²/day
@Thickness 0.100 mm,
Temperature 23.0 °C
0.966 g/100 in²/day
@Thickness 0.00394 in,
Temperature 73.4 °F
85% RH; ISO 15106-1
Oxygen Transmission 650 cc-mm/m²-24hr-atm1650 cc-mil/100 in²-24hr-atmcm³/(m²·24 h·bar), 100 µm film; b.o. ISO 2556
 2760 cc-mm/m²-24hr-atm7010 cc-mil/100 in²-24hr-atmcm³/(m²·24 h·bar), 25.4 µm (1 mil) film; b.o. ISO 2556
Nitrogen Transmission 120 cc-mm/m²-24hr-atm305 cc-mil/100 in²-24hr-atmcm³/(m²·24 h·bar), 100 µm film; b.o. ISO 2556
 510 cc-mm/m²-24hr-atm1300 cc-mil/100 in²-24hr-atmcm³/(m²·24 h·bar), 25.4 µm (1 mil) film; b.o. ISO 2556
Carbon Dioxide Transmission 3800 cc-mm/m²-24hr-atm9650 cc-mil/100 in²-24hr-atmcm³/(m²·24 h·bar), 100 µm film; b.o. ISO 2556
 16900 cc-mm/m²-24hr-atm42900 cc-mil/100 in²-24hr-atmcm³/(m²·24 h·bar), 25.4 µm (1 mil) film; b.o. ISO 2556
Linear Mold Shrinkage 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inparallel/normal; b.o. ISO 2577
Linear Mold Shrinkage, Flow 0.0070 cm/cm0.0070 in/in60x60x2 mm; 500 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0075 cm/cm0.0075 in/in60x60x2 mm; 500 bar; ISO 294-4
Melt Flow 3.0 g/10 min
@Load 1.20 kg,
Temperature 300 °C
3.0 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 65.0 MPa9430 psi50 mm/min; ISO 527-1/-2
Tensile Strength, Yield 67.0 MPa9720 psi50 mm/min; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Nominal, 50 mm/min; ISO 527-1/-2
 105 %105 %50 mm/min; ISO 527-1/-2
Elongation at Yield 6.4 %6.4 %50 mm/min; ISO 527-1/-2
Tensile Modulus 2.40 GPa348 ksi1 mm/min; ISO 527-1/-2
Flexural Strength 96.0 MPa13900 psi2 mm/min; ISO 178
Flexural Yield Strength 75.0 MPa
@Strain 3.5 %
10900 psi
@Strain 3.5 %
2 mm/min; ISO 178
Flexural Modulus 2.40 GPa348 ksi2 mm/min; ISO 178
Flexural Strain at Yield 7.1 %7.1 %2 mm/min; ISO 178
Izod Impact, Notched (ISO)  15.0 kJ/m²
@Thickness 3.00 mm,
Temperature -30.0 °C
7.14 ft-lb/in²
@Thickness 0.118 in,
Temperature -22.0 °F
complete break; ISO 7391/b.o. ISO 180-A
 60.0 kJ/m²
@Thickness 3.00 mm,
Temperature 23.0 °C
28.6 ft-lb/in²
@Thickness 0.118 in,
Temperature 73.4 °F
partial break; ISO 7391/b.o. ISO 180-A
Charpy Impact Unnotched NBNBISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
 NB
@Temperature -60.0 °C
NB
@Temperature -76.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.40 J/cm²
@Thickness 3.00 mm,
Temperature -30.0 °C
6.66 ft-lb/in²
@Thickness 0.118 in,
Temperature -22.0 °F
complete break; ISO 7391/b.o. ISO 179-1eA
 7.00 J/cm²
@Thickness 3.00 mm,
Temperature 23.0 °C
33.3 ft-lb/in²
@Thickness 0.118 in,
Temperature 73.4 °F
partial break; ISO 7391/b.o. ISO 179-1eA
Impact 55005500Puncture - maximum force (N); ISO 6603-2
 6400
@Temperature -30.0 °C
6400
@Temperature -22.0 °F
Puncture - maximum force (N); ISO 6603-2
Puncture Energy 60.0 J44.3 ft-lbISO 6603-2
 65.0 J
@Temperature -30.0 °C
47.9 ft-lb
@Temperature -22.0 °F
ISO 6603-2
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmIEC 60093
Surface Resistance 1.00e+16 ohm1.00e+16 ohmIEC 60093
Dielectric Constant  3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
IEC 60250
 3.1
@Frequency 100 Hz
3.1
@Frequency 100 Hz
IEC 60250
Dielectric Strength 34.0 kV/mm864 kV/in1 mm; IEC 60243-1
Dissipation Factor  0.0010
@Frequency 100 Hz
0.0010
@Frequency 100 Hz
IEC 60250
 0.0090
@Frequency 1e+6 Hz
0.0090
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 125 V125 VCTI M; Solution B; IEC 60112
 225 V225 VSolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
38.9 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
38.9 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1/-2
Thermal Conductivity 0.200 W/m-K1.39 BTU-in/hr-ft²-°Fcross-flow; ISO 8302
Hot Ball Pressure Test 115 °C239 °FISO 2039-1
 139 °C282 °FIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 139 °C282 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 127 °C261 °FISO 75-1/-2
Vicat Softening Point 146 °C295 °F50°C/h 50N; ISO 306
 147 °C297 °F50 N; 120 °C/h; ISO 306
Glass Transition Temp, Tg 146 °C295 °FISO 1133
UL RTI, Electrical 125 °C
@Thickness 2.00 mm
257 °F
@Thickness 0.0787 in
UL 746B
UL RTI, Mechanical with Impact 115 °C
@Thickness 2.00 mm
239 °F
@Thickness 0.0787 in
UL 746B
UL RTI, Mechanical without Impact 125 °C
@Thickness 2.00 mm
257 °F
@Thickness 0.0787 in
UL 746B
Flammability, UL94 V-0
@Thickness 2.00 mm
V-0
@Thickness 0.0787 in
IEC 60695-11-10
Flash Point 450 °C842 °FASTM D1929
 510 °C950 °FASTM D1929
Smoke Density 4.0 min4.0 min<200; ASTM E662
Oxygen Index 43 %43 %Method A; ISO 4589-1/-2
Glow Wire Ignition Temperature  875 °C
@Thickness 0.750 mm
1610 °F
@Thickness 0.0295 in
IEC 60695-2-13
 900 °C
@Thickness 1.50 mm
1650 °F
@Thickness 0.0591 in
IEC 60695-2-13
 900 °C
@Thickness 3.00 mm
1650 °F
@Thickness 0.118 in
IEC 60695-2-13
Glow Wire Flammability Index  960 °C
@Thickness 0.750 mm
1760 °F
@Thickness 0.0295 in
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
1760 °F
@Thickness 0.0591 in
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
1760 °F
@Thickness 0.118 in
IEC 60695-2-12
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5861.586Procedure A; ISO 489
Transmission, Visible  84 %
@Thickness 4.00 mm
84 %
@Thickness 0.157 in
ISO 13468-2
 85 %
@Thickness 3.00 mm
85 %
@Thickness 0.118 in
ISO 13468-2
 86 %
@Thickness 2.00 mm
86 %
@Thickness 0.0787 in
ISO 13468-2
 87 %
@Thickness 1.00 mm
87 %
@Thickness 0.0394 in
ISO 13468-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 310 °C590 °FInjection Molding; ISO 294
Mold Temperature 90.0 °C194 °FInjection Molding; ISO 294
Injection Velocity 200 mm/sec7.87 in/secISO 294
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 India
 Near East/Africa
 North America
 South and Central America
Eff. thermal diffusivity (m²/s)1E-07
FeatureLight stabilized or stable to light
 Release agent
 U.V. stabilized or stable to weather
FormPellets
ProcessInjection Molding
 Other Extrusion
UL recognitionUL\lh\n

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Makrolon® 6557 Polycarbonate, Injection Grade
Covestro Makrolon® 2865 Polycarbonate, Flame Retardant Grade
Covestro Makrolon® 2407 MAS056 Polycarbonate
Covestro Makrolon® 6455 Polycarbonate, Flame Retardant Grade
Covestro Makrolon® 6870 Polycarbonate

PB09936 / 92776

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.