MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex ELEXAR® EL 8431 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: Notes: Elexar® EL-8431 is a general purpose thermoplastic elastomer designed for electrical applications requiring flexibility over a wide temperature range. Elexar® EL-8431 is a low density, medium hardness, RoHS compliant grade suitable for both injection molding and extrusion.

Features: General Purpose; Good Colorability; Good Flexibility; Halogen Free; High Elasticity; High Elongation; High Tensile Strength; Low Density; Low Flow; Low Temperature Flexibility; Low Temperature Toughness; Medium Hardness; Ozone Resistant; Sunlight Resistant (720 hours); UV Resistant; Weather Resistant

Uses: Appliance Wire Insulation; Appliance Wire Jacketing; Cable Jacketing; Connectors; Flexible Cord Jacketing; Industrial Cable Insulation; Terminal Cable Jacketing; Underground Power Cable; Wire & Cable Applications; Wire Jacketing

Automotive Specifications:FORD ESB-M2D296-A

Form: Pellets

Processing Method: Extrusion; Injection Molding

Information provided by Teknor Apex Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.922 g/cc0.922 g/ccASTM D792
Melt Flow 6.0 g/10 min
@Load 5.00 kg,
Temperature 230 °C
6.0 g/10 min
@Load 11.0 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6969ASTM D2240
Tensile Strength, Yield 17.2 MPa2500 psi0.02 in, Die C, 20 in/min, die cut from extruded tapes; ASTM D412
 14.1 MPa
@Treatment Temp. 60.0 °C,
Time 605000 sec
2050 psi
@Treatment Temp. 140 °F,
Time 168 hour
in IRM 902 Oil; ASTM D471
 17.41 MPa
@Treatment Temp. 136 °C,
Time 605000 sec
2525 psi
@Treatment Temp. 277 °F,
Time 168 hour
in Air; ASTM D573
Tensile Stress at Strain  2.48 MPa
@Strain 100 %,
Thickness 0.508 mm
360 psi
@Strain 100 %,
Thickness 0.0200 in
Die C, 20 in/min, die cut from extruded tapes; ASTM D412
 4.52 MPa
@Strain 300 %,
Thickness 0.508 mm
655 psi
@Strain 300 %,
Thickness 0.0200 in
Die C, 20 in/min, die cut from extruded tapes; ASTM D412
Elongation at Break 710 %710 %0.02 in, Die C, 20 in/min, die cut from extruded tapes; ASTM D412
 667.4 %
@Treatment Temp. 60.0 °C,
Time 605000 sec
667.4 %
@Treatment Temp. 140 °F,
Time 168 hour
in IRM 902 Oil; ASTM D471
 681.6 %
@Treatment Temp. 136 °C,
Time 605000 sec
681.6 %
@Treatment Temp. 277 °F,
Time 168 hour
in Air; ASTM D573
Flexural Modulus 0.0379 GPa5.50 ksiASTM D790
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 9.10e+16 ohm-cm9.10e+16 ohm-cm122°F; ASTM D257
Insulation Resistance 1.00e+12 ohm1.00e+12 ohmIEC 60167
Dielectric Constant 2.1
@Frequency 1000 Hz
2.1
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 38.2 kV/mm970 kV/inASTM D149
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 105 °C221 °FContinuous; UL-1581
Brittleness Temperature <= -100 °C<= -148 °FASTM D746
UL RTI, Electrical 90.0 °C194 °FUL 746
UL RTI, Mechanical with Impact 90.0 °C194 °FUL 746
Flammability, UL94 HB
@Thickness 0.762 mm
HB
@Thickness 0.0300 in
All Colors
Oxygen Index 18 %18 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 199 - 216 °C390 - 420 °F
Middle Barrel Temperature 213 - 221 °C415 - 430 °F
Front Barrel Temperature 221 - 227 °C430 - 440 °F
Nozzle Temperature 221 - 229 °C430 - 445 °F
Zone 1 193 - 210 °C380 - 410 °F
Zone 2 199 - 216 °C390 - 420 °F
Zone 3 213 - 221 °C415 - 430 °F
Zone 5 221 - 227 °C430 - 440 °F
Die Temperature 221 - 229 °C430 - 445 °F
Melt Temperature 221 - 229 °C430 - 445 °FProcessing Temp
Mold Temperature 25.0 - 65.6 °C77.0 - 150 °F
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Elexar® EL-8431 Thermoplastic Elastomer
Teknor Apex ELEXAR® EL 8451 Thermoplastic Elastomer
Teknor Apex Elexar® EL-8451 Thermoplastic Elastomer
Teknor Apex ELEXAR® EL 8730 Thermoplastic Elastomer
Teknor Apex Elexar® EL-8730A Thermoplastic Elastomer

PTEKNO261 / 70004

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.